Re: [MW:35786] Request for Guidance on PQR Update

Please refer to ASME sec IX - QW-200.2 & QW-401.1.

While ASME IX does not explicitly use the term "supplementary PQR", industry practice is to weld a new coupon 

with the same WPS variables, which is issued as a new PQR; i.e., one cannot add hardness test results to the original 

PQR, because that would not represent the same coupon. You must weld a new coupon and issue a new PQR with 

hardness results, and cross-reference the original PQR if traceability is required.


C Sridhar.


On Fri, 29 Aug 2025 at 11:49, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
is there any ref in code, pl share it

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Thu, Aug 28, 2025 at 6:20 PM sridhar cn <sridharcn305@gmail.com> wrote:
You need to write in the new supplementary PQR format as the hardness testing date is current.
Since the old PQR results (other than hardness values- as per the standard) are the same, it is not necessary 
to enclose the old PQR. But, if your client insists, please act to satisfy him.
C Sridhar.

On Thu, 28 Aug 2025 at 13:34, sridhar cn <sridharcn305@gmail.com> wrote:

You can make a new, "Supplementary PQR" as it is safer and cleaner from a compliance and transparency 

standpoint. You prepare a new PQR document with all the welding parameters repeated from the original PQR,

plus the new hardness test results.

            

You can add a note referencing the original PQR number (i.e., "This PQR was performed under the same welding

conditions as PQR-001 (provide actual details) to incorporate the hardness testing per client requirements").


C Sridhar.


On Thu, 28 Aug 2025 at 12:21, pankaj pachahara <pankajpachahara@gmail.com> wrote:
Dear Experts,

We have a qualified PQR (P1 to P8) that doesn't include hardness testing. We're submitting this PQR for a new project, but the client requires hardness testing. To address this, we plan to:

1. Create a new PQR following the same parameters as the original PQR.
2. Conduct hardness testing and add the results to the new PQR.

We're unsure about the best approach to incorporate the hardness test results into our existing PQR documentation. We have two options:

Option 1- Add the hardness values to the original PQR as Addendum-1.
Option 2- Create a new PQR that includes all the previous data and name it as a Supplementary PQR.

Could you please guide us on the best approach to take?

Best regards
Pankaj Choudhary

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJF_nWPufvGG-sFFjNLMxN8QYd3Dqo4DHA%2B8r_ocT1_7A2SbFA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYih3EbLXznCG5Cb9-c6Sa%2B_z1T8fChrE1%2BZx9Z9rrJk-8Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eM68D5VYocP2qb-NM7osefhAFbd_cENPpwTV7YfegCXgg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYihZqSvaVkL1GqKnWjmVQ%3Dt6XM6K769t70%2Bb6riFiVpTzQ%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...