Re: [MW:35743] PQR- Chemical testing requirements

For your 2-inch 8 mm thick CS pipe welded, as per ASME Sec. IX standard, you require:
Visual examination,
2 Tensile tests, 
2 each in the face and root bends.
No hardness, impact  and chemical tests are required. 
Use the MTC of the base metal if required.
Micro/Macro are required for Fillet weld only.
C Sridhar.
---------------------------------------------------------------------------------------------------------------






On Fri, 1 Aug 2025 at 16:58, kingslygeo vargheese <kingslygeotech@gmail.com> wrote:
Good Day to all,

Reference std: ASME SEX IX

Material ASTM A106 Gr B

Pipe Dia and thickness: 2" and 8.74 mm.

Service Fluid: Normal fluid

as per the Standard ASME SEX IX ( no client/company specification involved )

1. What are the minimum testing requirements to qualify the PQR?

2. Is chemical testing required or not?

Thanks 

Best Regards
V.Kingsly Geo




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAAR7VZ823gnF3g%3DcB6gpwrTKAkOGX5EwNU-c8vh0SoQkSjMw5w%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiBNyD2uUd-5Z58tc9EKRRetUPqEDL-s8jqdb8JVF8Anw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .