Re: [MW:34133] Suggestion for welding consumable

You can try EA2 wire with suitable Flux in the stress relieved condition by consulting with Welding consumable supplier

Thanks & Regards

J.Gerald Jayakumar




On Thursday, 13 April, 2023 at 08:43:32 am IST, SMM <sohilmehta@gmail.com> wrote:


Dear Mr.Jayakumar, 

Thank you for the reply. 

Please advise which consumable can be used for SAW welding

Can EH12K and combination flux be used. ??

On Tuesday, 11 April 2023 at 08:46:03 UTC+5:30 james gerald wrote:
I suppose it is a DE weld. Use 90ksi electrode/Filler Rod as after Normalizing there will be 15-20ksi loss in Tensile strength

Thanks & Regards

J.Gerald Jayakumar



On Monday, 10 April, 2023 at 10:34:38 am IST, Sohil Mehta <sohil...@gmail.com> wrote:


Dear Experts, 


Kindly suggest consumables for below 


Material SA516GR70

Impact @-40C

Impact values – 27J min

 

Normalizing

Loading – 300C

ROH – 150C

Soaking Temp – 900-920

Soaking Time – 80min

Still Air

 

SR

Loading – 300C

ROH – 50C max/hr

Soaking – 625C- 645C

Time – 720mins

ROC – 65C max / hr upto 425C


Thank you.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8046052f-73a0-46dd-9523-d130fd6069d8n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/83385312-73ea-474b-8154-f1bae97ac890n%40googlegroups.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...