Re: [MW:33425] Pickling and passivation need before painting SS surfaces

Due to Stellite-6 / 21  overlay, the Heat transfer will be there in the SS part also.

1. Internal PP is required.
2. Based on the above External PP may get a waiver from the Client,

On Fri, 29 Jul 2022 at 11:53, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Normally in the seat they apply stellite overlay  which is cobalt based for wear resistance. Only stainless steel can be pickled and passivated.


On Fri, 29 Jul 2022 at 7:59, Anilkumar G
Dear Experts

Thanks all for very valuable support. 

There is an overlay welding involved in the body seat of the valve. Do we need pickling and passivation inside only in this case?

Outside there will be painting. 

Regards
Anilkumar

On Thu, Jul 28, 2022 at 9:18 AM Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
Sweep sand blast and do painting, Pickling & Passivation not required
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Thu, Jul 28, 2022 at 8:55 AM Sudhakar Kuppuswamy <sudhakarceng@gmail.com> wrote:
If the painting is applicable , picking and passivation is not required.

Regards,
Sudhakar K 

On Tue, 26 Jul 2022 at 12:19 PM Anilkumar G <akg.nitt@gmail.com> wrote:
Dear Experts

Do we need pickling and passivation of SS surfaces before painting them? Could you please suggest any specification relevant this requirement?
The parts are SS cast valves requiring painting.

Regards

Anilkumar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/754e0d61-54e1-420e-ae4b-f92593266f5en%40googlegroups.com.
--

Regards,

Sudhakar K CEng MWeldI,IWE.

Welding & Metallurgical Engineer,

Email: sudhakarceng@gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABF8NYWeTdW37oKU%2BwEVKNmUahae9_1vrYA5XfvizQou11HzYg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eP86mvMhpBPm_vf5H4P2nq_pqXfkT5gS3tCd8vAcF0sdw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKMJiNVymuU1embz2s-Yt%3DQfW9pzALNx%2BVH-oh%3DY4cKqzHTvEQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1975556184.2090738.1659076464852%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAR7VZ8DU%2BBGRqDtknaVuQDXcfMQ-jAPd4anrN3af%3DAK8KHDOw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...