Skip to main content

Re: [MW:33399] Re: Weld Copper to Stainless Steel 304

My opinion with experience Copper to SS welding is not compatible
You can braze or vaccine braze with BAg8 or similar  filler
Hegde


On Thu, 25 Aug 2022 at 18:04, 'J Prinsen' via Materials & Welding
<materials-welding@googlegroups.com> wrote:
You can try with inconel 625 or Nickel 200, or buttering the stainless steel with either 625 or 200 and then weld with the same consumable  to the copper
I' ve seen welding with a copper consumable in the past, but there is a high risk of hot cracks


Regards

Jurgen Prinsen IWE

Van: "Mohd Siraj" <mohd52100@gmail.com>
Aan: "materials-welding" <materials-welding@googlegroups.com>
Verzonden: Donderdag 11 augustus 2022 17:09:48
Onderwerp: [MW:33377] Re: Weld Copper to Stainless Steel 304

pl share exact specification of material to be weld with thickeness.
for any question to be answered quickly , you could provided suffiecent details so that other can understand your requirement like code interpretation querry.

On Saturday, July 30, 2022 at 5:00:55 PM UTC+3 Sohil Mehta wrote:
Dear Sir, 
Kindly suggest consumables for welding of Copper to Stainles Steel. 
Thank you.

Regards,
Sohil Mehta

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c84d8a39-6385-4d7d-9c48-df32d4658770n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2056395243.42875647.1661429976858.JavaMail.zimbra%40online.nl.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1295258517.2205182.1661433554582%40mail.yahoo.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...