Thursday, April 15, 2021

Re: [MW:32256] welding api 5l x52 with x60


As per API 1104 , 2013 edn, Clause 5.4.2.2 , you can use the same WPS without requalification. I presume your flange and fittings are having same SMYS ( Specified Minimum Yield Strength)  and similar CEq

 

Requalification is required only when the base metal welding involves less than X42 or greater than X65. In your case this is not applicable.

 

Make sure, Your WPS have mentioned : Qualified Base material X42 Through  X60.

 

            Keeping future qualification purpose, it's better to qualify PQR with X65 material which many customers accept for all lower grades' base metal qualification.

Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Thu, Apr 15, 2021 at 1:08 PM QA/QC <adnanziad49@gmail.com> wrote:
Dear master 
i have a approved wps for welding api 5l x52  pipeline and i want to weld a anchor flange x60 is the wps cover it or we should requlaify it again 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c82adcc6-aec4-4acc-9815-966de7fd1a23n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcE4RSSTrs_hiOJX%2ByyRx28Uu0yXGx_j5dTa74%2BG-_BYcA%40mail.gmail.com.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...