Hi Prem,

 

These alloys are really special type of alloys. Precipitation hardenable hence all alloys have to be aged after welding . Different aging temperatures are applicable according to the specifications and required properties. I've highlighted the nominal mechanical properties in SA-564 ,extract as attached.

Typically, E 630 electrodes/filler metals are used for welding 17/4ph stainless steel. This grade is most commonly used PH stainless steels , in valves and other components.

If matching Turballoy 13-8 welding consumable is not available by any means, 17/4 ph or E/ER 630 electrode/filler metal would be the way to go.

 

If E630 does not meet the criteria, consumables for Precipitation hardenable Nickel Based alloys would be the only available  option.

 

Regards.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Prem Nautiyal
Sent: April 20, 2021 10:58 PM
To: materials-welding@googlegroups.com
Subject: [MW:32319] Suitable filler wire for UNS S13800/ ASTM-A 705 Gr XM-13 PH 13-8 Material

 

 

Dear All

 

We need expert advice on best suitable filler wire and Welding process for following base  material - 

 

Base Material :  AISI/ UNS S13800/ ASTM-A693/ A 705 Gr XM-13  PH 13-8

   

Chemical Requirements of base material: 

 

Carbon 0.05 

Manganese 0.2 

Phosphorus 0.01

Sulfur 0.008

Silicon 0.1

Chromium 12.25 to 13.25

Nickel 7.5 to 8.5

Aluminum  0.9 to 1.35

Molybdenum 2 to 2.5

 

 

  Base material thickness 8 to 16mm thk..  

   

  1)  Welding Process :  TIG or SMAW

   

  2) Joint geometry : Butt Weld (Full penetration joint)  

  3) Age hardening to be done after welding  

  4) After age hardening UTS shall be 1520 Mpa min, YS = 1420 MPa, El= 10%.  

  5) After age hardening hardness required 45 HRC minimum  

 

 

We have selected one TIG filler wire Turballoy 13-8 Mo which matches the chemical composition of our base material and has same UNS Number. The manufacturer is United States Welding Corporation but not available in India..

We have past experience of 15-5 PH stainless steel welded with ER 630 Filler wire but UTS achieved after age hardening is 1100 MPa.

Also some reputed consumable manufacturers have suggested ER 630 filler wire but cannot guarantee strength and hardness after age hardening.

 

We would like to know the suitable filler wire / electrode and best process to weld this material - TIG / SMAW.

Regards

 

Prem Nautiyal 

Cell 9082354678 / 9082354678

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEP2HKAc6iCuSmTNzPBmzM4Je1Krwd8O2Z%2B-%3DAqJ3Kz7rmQeKA%40mail.gmail.com.


Virus-free. www.avg.com

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...