Monday, February 12, 2018

Re: [MW:27332] P-22 plate welding ...6-MM plate

Hi ! 
Probable causes
a post heating say.300 to 350 c
b baking of electrodes properrly in oven say at 300 to 350 c with adequet holding time
c check bead thk.Should not be excessive
d distortion of jt.during.welding
Regards

Hegde


On Sun, 11 Feb 2018 at 16:42, pradip kumar Sil
<pradipsil@gmail.com> wrote:
Dear Everybody,

We are doing  P-22 plate welding, thickness is 6 mm with E-9018B3 ( Dia 2.5 mm) electrode. Preheat is 150 to 200 degree centigrade with little beveling. Site is near the sea area.

We found lot of delayed crack  generally after 12 hours. Crack is coming middle of the weldment.

Can anybody inform me cause & corrective action for the same. 

Pic attached for your ready reference.

Thanks in advance.
Regards,

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...