Friday, June 26, 2015

Re: [MW:23118] welding 4340 to A36

Hamid jaan ..

Kindly recommend to care about pre- heating for minimum 300°F and maximum interpass around 600 °F ,after welding cover/wrap it by proper heat reaistant blanket so that it cool down slowly.
For PWHT just look at the MTR or mill maker recommendation. However be aware that holding temp is around 1000°F usaully.

After stress relief MPI is recomanded.

Regards
~Reza

On Jun 25, 2015 10:30 AM, "Hamid Firoozi" <h.firoozi61@gmail.com> wrote:
Hello Experts

We are going to welding 4340 to 1020 with FCAW . I know 4340 has potential for Cracking after welding ,so i`m looking for advise on welding and PWHT and backing during and after finished job

4340 in our part is with Normalized and tempered  . and no quench on it based on customer spec to catching specific hardness.

please share your experience  with me.

Thanks all

  

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ee9a24a0-ceba-4332-9223-3052984a4b32%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANOFoyjrPhA%2ByC846KUfoKQ8%2B6DBODL8viz3uzT9%3Dv-hYZo3-w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...