Dear Venkat
As per ASME Sec VIII Div-1 UCS-56 Notes-2(C)you can preheat to a minimum
temperature of 200Degree F(95degC)is applied and weld both nozzle if have
WPS is available. If you can applied preheat you can avoid PWHT for both
nozzle.
With regards,
Jatin
-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
g.venkatesan06@gmail.com
Sent: Friday, October 26, 2012 8:54 AM
To: materials-welding@googlegroups.com
Subject: [MW:15768] Requirement of PWHT in categorie D
Dear sir.
Kindly replay the below mail
regards
venkat
----------
Sent from my Nokia phone
------Original message------
From: g.venkatesan06@gmail.com <g.venkatesan06@gmail.com>
To: "materials-welding@googlegroups.com"
<materials-welding@googlegroups.com>
Date: Thursday, October 25, 2012 2:56:08 PM GMT+0000
Subject: Requirement of PWHT in categorie D
Dear experts,
we are doing welding in a vessel of joint nozzle to dish with reinforcement
pad(pipe thick 10mm(32inch), dish thik 20mm & RF pad 20mm) the weld detail
in drawing shows bevel(55 degree) followed with fillet(10mm). All are P1
material.
In my question : the total weld metal deposit is 50mm in a joint(40mm CJP &
10 Fillet)
code says above 38mm groove weld for P1 material PWHT is mandatory and also
says groove & fillet exceed 26mm in 2inch pipe PWHT is required.
Now we will do PWHT or not in a particular joint. If not kindly tell the
reason.
Regards
venkat
welding engineer
trichy.
----------
Sent from my Nokia phone
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=
anet_ug_hm
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Subscribe to:
Post Comments (Atom)
[MW:35668] Selection of Filler/Electrode.
Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment