hi,
it will be straight under lower mag and same will be in zig-zag/tapered in both direction under high mag.
each zig-zag point connects to make a straight line(H .mag).
under low mag u can see zig-zag only if the residual/ service stress is high enough to reveal it and it will be not straight at normal mag.



On Sun, May 29, 2011 at 2:24 PM, sajidalam mohd. <engineer_makes_world@yahoo.co.in> wrote:
DEAR EXPERTS
                     GOOD DAY
CAN ANY ONE EXPLAIN HOWS CRACKS IN WELD ON X-RAY FILMS LOOKS?
 
IT LOOK LIKE ZIZ ZAG???
ITS LOOKS LIKE THIN/NARROW STRAIGHT LINE???
 
BECAUSE I AM  CONFUSED ABOUT INDICATION OF CRACKS OF WELDING ON X-RAY FILM?
 
 
WAITING FOR REPLY.
 
REGARDS
MOHAMMAD SAZID ALAM
INSPECTION ENGINEER
AICO-DAMMAM
MOBILE:-0534077860

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
_____________________________________________________________________________________

C . R . RATHOD
PhD Student
SCHOOL OF MECHANICAL,MATERIALS & MECHATRONIC ENGINEERING
SMART BLDG 6,  ROOM NO: 107
UNIVERISTY OF WOLLONGONG - 2522
NEW SOUTH WALES 
AUSTRALIA

M   : +61434059865
P    : 04239 2356

______________________________________________________________________________________

Minds are like parachutes - they only function when open. - Thomas Dewar
_____________________________________________________________

If you do not understand my silence, you will not understand my words
_____________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...