Dear all,

First of all lets go one by one

stage-1 material inspection stage:
if these pitting have gone overlooked during incoming inspection then
it was really serious issue and even AI also didnt noticed.!!!

Refer UG-16(2) and as you said 3mm is corrosion allowance then it is
0.50mm is acceptable.if need UT to be done to get actual thickness
sorrouding area and deviation/concession note to be raised and Aproved
by AI.

Stage-2 fabrication stage:

if these things happend due to any atompheric effect/fabrication

Refer UW-32(a),/UW-35(1) (2) for acceptance.

in all case involvement of AI is mandatory.

if go depth..then u wil have to prepare repair procedure followed by
approved WPS prior commence any any repair!!!

On May 27, 9:44 am, asad azmi <azmiasada...@gmail.com> wrote:
> Dear All,
>
> Greetings.
>
> Pittings (not more than 0.5 mm in depth) observed on the surface of a shell
> of a Vessel. pls find photos for your reference.
>
> Shell material  is SA 36. thickness 8mm. service fluid - water
>
> Code of construction is ASME SEC VIII DIV1
>
> After grindings also pittings can be observed on the large surface of the
> shell.
>
> *Whether these pittings can be accepted as it is OR further grinding is
> required.*
>
> Please Suggest.
>
> Thanks and Regards
>
> Asad Azmi
>
>  2605201111622.jpg
> 568KViewDownload
>
>  2105201111425.jpg
> 666KViewDownload
>
>  2105201111426.jpg
> 556KViewDownload
>
>  2605201111620.jpg
> 785KViewDownload
>
>  2605201111621.jpg
> 758KViewDownload

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...