Skip to main content

Re: [MW:6164]Transverse Crack

Nilesh :

Did the plate undergo certain cold working process (rolling,bending,etc) prior to welding ? if so it would likely due to residual stress that cause the cracking, you could try to prolonge the preheat time and see if it still cracking or not

Also I found that the cracking susceptibility increases with an increase in the welding current, and decreases with an increase in the welding speed or the electrode wire feed rate. It also increases with increases in the plate rolling reduction ratio .

Regards
Richard Napitupulu
JWES Certified Welding Engineer CWEng
QA/QC Site Representative Pertamina Hulu Energy
Offshore West Java



From: "GERING, Erwin" <Erwin.GERING@airliquide.com>
To: materials-welding@googlegroups.com
Sent: Wed, 28 July, 2010 1:12:25 PM
Subject: [MW:6161] RE: 6154] Transverse Crack

Mostly these crackings are related to hydrogen.

Can you please specify filler metal (wire – flux combination) and hydrogen precautions (redrying?) and thickness.

 

 

With kind regards, mit freundlichem Grüss, salutations, met vriendelijke groet,

 

Ing. Erwin GERING, IWE

 

Corporate Product Manager      - ALW-corp. mktg           - SAW Wire & Flux        

Product Manager                           - ALW-NL & BeLux          - Welding Consumables                                            

(Tel.: 31(0)76 – 54 83 222  ÃˆMob.: 31(0)6 - 55 87 29 21

Air Liquide Welding_RVB_5.jpg

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens waman nilesh
Verzonden: dinsdag 27 juli 2010 18:58
Aan: materials-welding@googlegroups.com; materials-welding@goolegroups.com
Onderwerp: [MW:6154] Transverse Crack

 

I want to know the exact cause off transverse crack observed visually on the surface of the weld.

 

Welding done with SAW 

Material - SA 516 GR. 70

Thickness- 32 mm

We have done pre heating at temperature 100 deg. C but from top side also check the filler wire material 

after crack are observed which are ok.

Please share your experience with me on this issue.

Regards,

Nilesh

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...