Re: [MW:6140] Re: Welding of ASTM A 335Gr.P11

Dear All,
 
Thank you verymuch for the valuable inputs.
 
@Manpreet,I would like to know more about bare electrode usage and temper bead technique in depth.
 
What is the difference between temper bead technique and normal welding technique?
 
Is there any different sequence of layering technique we are following in temperbead ?
 
If so how we can ensure it always since the welders are not much bothered about systematic layering? 
 
If you don't mind please share some presentation or simulation on temperbead technique.
 
 
Thanks and Regards,
 
 
Limesh
 


 
On Tue, Jul 27, 2010 at 10:19 AM, manpreet <manpreetsin88@rediffmail.com> wrote:

Dear All

Completely agree with Mr, Hegazy.

Mr. limesh, there is nothing as such E7018 B2 (E7018 B2L is available).

ASME SECii part c, the best suitable covered electrode is E8018 B2, which you can use without PWHT with temperbead technique.

If you want to use the bare electrode or info regarding temperbead technique,Pls let me know.

Regards
Manpreet Singh
Welding Engineer
SpiecaPag LPG-LNG Project



On Sat, 24 Jul 2010 23:27:01 +0530 wrote

>i have specified "not E-7018B2" in my reply since it is not listed in

AWS classification. only 8018B2 is listed in addition to 7018B2L.

there is no restriction on use of both of these grades.



On Jul 24, 12:32 pm, MOHAMED HEGAZY wrote:

> Dear Raghuram,

>

> I Believe that as strenght point of view it's ok to use E7018B2L but why i have to go for this low carbon grades while there is no need for that specially that the base metal itself has a 0.05 to 0.15 %C range which will be higher than weld metal and conequently may cause carbon to migrate from HAZ to the weld metal resulting in embrittling effect & in case of high operating temperature this carbon is highly required to stablize the the chromium atoms in the weld metal to avoid loosing the strenght & creep resistance at high temperatures.

>

> So I recommend not to go for E7018B2L & as long as there's no E7018B2 so E8018B2 is more matching for this case .

>

> Another points of view are encouraged.

>

>

>

>

>

>

> Regards

>

> Mohamed.Hegazy

> F.S.I Coordinador

> PgDip of Welding Engineering

> AWS Certified Welding Engineer CWEng.

> TWI CSWIP Welding Inspection 3.1.

> VSA Consortium ( VEOLIA, SAIPEM & ALJABER )

> Power & Energy Projects.

> QATAR SHELL PEARL GTL Project.

> Ras Laffan ,Qatar

>

> QATAR :+9743694501

> EGY: +20142345614

> Email :MH_w_INSP...@YAHOO.COM

>

>

> --- On Thu, 7/22/10, Raghuram Bathula wrote:

>

> From: Raghuram Bathula

> Subject: Re: [MW:6084] Welding of ASTM A 335Gr.P11

> To: materials-welding@googlegroups.com

> Date: Thursday, July 22, 2010, 5:50 PM

>

> you can use E-7018B2L (not E-7018B2). the "L-Grades" are limited to a maximum of 0.05% carbon. While the lower percent carbon in the weld metal will improve ductility and lower hardness,it will also reduce the high-temperature strength and creep resistance of the weld metal.

>

> Generally it is not a problem with P11, but in case of P22 if the operating temp is > 450 °C, one must not use low carbon grades

>

> On Thu, Jul 22, 2010 at 6:21 PM, limesh M wrote:

>

> Can we use E-7018B2 instead of E-8018B2 for welding of A-335 Gr. P11

> material. If yes then what care shall be exercised during welding?

> Would the resulting weldment be of adequate strength?

>

> Thanks and Regards

>

> Limesh

>



--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...