Note that materials No 1.429 & 1.4740 arn't cast iron,

Material Number
1.4729

Steel group
Stainless and heat-resisting steels

Symbol
GX40CrSi13

Standards
?NORM EN 10295 (10/2002)
Heat resistant steel castings

Range of application
Heat-resisting steel castings:
Hearth-plates, door frames and other similar hearth parts.
Suitable welding filler materials 1.4733, 1.4829.

Material Number
1.4740

Steel group
Alloy special steels: Heat resistant steels with < 2,5% Ni

Symbol
GX40CrSi17

Standards
DIN EN 10295 (01/2003)
Heat resistant steel castings
International conformity
EN 10295 (2002)
Replaces
DIN 17465 (08/1993)

Range of application
Heat-resisting steel castings:
Superheater parts, pipe clamps, carrying handles, grates.
Suitable welding filler materials 1.4015, 1.4502, 1.4829.

Material Number
1.1191

Steel group
Non alloy special sructural steels: Structural steels with average C <
0,50%

Symbol
C45E; Ck 45 †

Standards
DIN EN 10083-1 (10/1996)
Quenched and tempered steels. Special steels.
International conformity
EN 10083-1+A1 (1996)
Replaces
DIN 17200 (03/1988) (03/1987)

DIN EN 10132-3 (05/2000)
Cold-rolled narrow steel strip for heat-treatment. Steels for
quenching and tempering.
Replaces
EN 10132-3 (2000)

DIN EN 10250-2 (12/1999)
Open die steel forgings for general engineering purposes. Non-alloy
quality and special steels.
Replaces
EN 10250-2 (1999)

DIN EN 10269 (11/1999)
Steels and nickel alloys for fasteners with specified elevated and/or
low temperatures properties.

DIN EN 10277-5 (10/1999)
Bright steel products. Steels for quenching and tempering.

DIN EN 10297-1 (06/2003)
Seamless circular steel tubes for mechanical and general engineering
purposes. Non-alloy and alloy steel tubes. Non-alloyed high-quality
steels

DIN EN 10297-1 (06/2003)
Seamless circular steel tubes for mechanical and general engineering
purposes. Non-alloy and alloy steel tubes. Alloyed quality steels

DIN EN 10305-1 (02/2003)
Steel tubes for precision applications. Seamless cold drawn tubes.

DIN SEW 550 (08/1976)
Steels for larger forgings.

Range of application
Heat-treatable steels:
Automobile- and motor construction, mech. engineering

High-temperature constructional steels:
Bolts and nuts, resistant to elevated temperatures up to 400 °C

These steels can also be supplied with a sulphur-content of
0,020-0,040%. Then e.g. C22E = C22R, resp. Ck22 = Cm 22 or receive the
letter S (e.g. 32Cr2 = 32CrS2). Number of material in brackets. The
mechanical properties are identical.

Material Number
1.0570

Steel group
Non alloy quality steels: Steels with average C > 0,25 < 0,55 % or Rm
> 500 < 700 N/mm²

Symbol
S355J2G3; St 52-3; St 52-3 G; (S355J2G3+CR)

Standards
DIN 1623-2 (02/1986)
Steel flat products. Cold reduced sheet and strip. General structural
steels.
International conformity
ISO 4997 (1999)

DIN 5512-1 (05/1997)
Materials for rail vehicles. Structural steels and structural steels
with improved atmospheric corrosion resistance, hot rolled.

DIN 5512-2 (05/1997)
Materials for rail vehicles. Unalloyed steels for cold rolled flat
products up to 3 mm thickness.

DIN 5515 (11/1978)
Steel sections, bars and flat products of non-alloyed steels and
general structural steels. Summary for rail vehicles.
Replaced by
E DIN 5515 (10/1999)

DIN EN 10025 (03/1994)
Hot rolled products of non-alloy structural steels.
Replaced by
EN 10025 (1993); ISO 630 (1995); ISO 4995 (2001); ISO/FDIS 6316
(2000); ISO 13976 (1998)

DIN EN 10250-2 (12/1999)
Open die steel forgings for general engineering purposes. Non-alloy
quality and special steels.

Way of deoxydation: Fully killed steel containing nitrogen binding
elements in sufficient amounts to bind the nitrogen (p.e. Al >=
0,02%).
With special cold workability: 1.0569; S355J2G3C
Former designation DIN 17100: St 52-3 N
Former designation of steels with special working properties,
Cold flanging: 1.0573; QSt 52-3 N
Cold drawing: 1.0597; ZSt 52-3 N
Cold roll forming: 1.0575; KSt 52-3 N

Material Number
1.0569

Steel group
Non alloy quality steels: Steels with average C > 0,25 < 0,55 % or Rm
> 500 < 700 N/mm²

Symbol
S355J2G3C; QSt 52-3

Standards
DIN 5512-1 (05/1997)
Materials for rail vehicles. Structural steels and structural steels
with improved atmospheric corrosion resistance, hot rolled.

DIN EN 10025 (03/1994)
Hot rolled products of non-alloy structural steels.
International conformity
EN 10025 (1993); ISO 630 (1995); ISO 4995 (2001); ISO/FDIS 6316
(2000); ISO 13976 (1998)
Replaces
DIN 17100 (01/1980)

DIN EN 10277-2 (10/1999)
Bright steel products. Steels for general engineering purposes.

Material Number
1.0576

Steel group
Non alloy quality steels: Steels with average C > 0,25 < 0,55 % or Rm
> 500 < 700 N/mm²

Symbol
S355J2H; RoSt 52-3

Standards
DIN 1626 (10/1984)
Welded circular unalloyed steel tubes subject to special requirements.
International conformity
ISO 9330-1 (1990)
Replaces
DIN 1626-1 (01/1965); DIN 1626-3 (01/1965)

DIN EN 10210-1 (09/1994)
Hot finished structural hollow sections. Non-alloy steels

DIN EN 10219-1 (11/1997)
Cold formed welded structural hollow sections. Fine grain steels

Material Number
1.0976

Steel group
Alloy quality steels: Steels for various applications

Symbol
S355MC

Standards
DIN EN 10149-2 (11/1995)
Hot rolled flat products made of high yield strength steels for cold
forming. Delivery conditions for thermomechanical rolled steels.
International conformity
EN 10149-2 (1995); ISO 5951 (2001); ISO 6930-1 (2001)

Range of application
Fine grained steels for cold pressing:
Longitudinal beams
Construction of frames
Parts for cold pressing
Cold rolled sections

On Jun 11, 10:25 am, limesh M <limes...@gmail.com> wrote:
> Dear All,
>
> I am in urgent need of theequivalentstandards of the following
> materials(From which standards these designated materials came) for
> chemical composition and traceability.Please help me .
>
> Cast Iron                       1.4729
>
> Cast Iron                       1.474
>
> Flat Iron                        C45K
>
> Cast Iron                      ENGJL250
>
> Cast Iron                      ENGJL250+1.5% CR
>
> Shaft                            S355J2G3
>
> Shaft                            S355J2G3+C
>
> Pipe                             S355J2H
>
> Steel Plate                   S355MC
>
> M16 Hex Bolt               DIN 916
>
> 17 Washer                   DIN 7349
>
> Refractory                    Alocast H 40
>
> Thanks &Regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...