Re: [MW:3919] the substitute NDT

Dear Eng. Mostafa,
If you wants the permanent record as it is the requirement of ASME Sec. VIII Div. 2 ....................
You have following two choices.
1. RT with CO 60 - Since It seems available to and fullfill ther requirement of Code.
As you mentioned you are worried about ineficiency of RT for 80mm.
You can do manual UT 100% weld length as per ASME section V - Article 4 prior to RT.
You can surely find all type of defects like Lack of fusions, cracks, Slags.
If the detected defects not acceptable in UT get them repaired. And for code requirement you can do RT for permanent Record.
 
2. Auto UT ToFD or Phased Array is the best choice for it and accepted by Code case 2239.
It may expensive and as you mentioned not easily available. If your job quantity is more you will get it and may be it will cheaper for you. But in this case you should find a company finalise the financial matters and then get the AUT procedure approved for your job. Qualification of AUT procedure is required. I can help you to find the NDT company providing the AUT services and write up the ToFD procedure. Contact me in this regards.
 
These are the two options.
 
Best Regards,

Nilesh Pathare.

 
On Wed, Dec 30, 2009 at 1:55 PM, Eng/ Mostafa Kamel Hussein <mkh_200@yahoo.com> wrote:

I have material with 80mm thickness and it's known that RT is not applicable for application as NDT, so what is the substitute method for NDT and please give me the code case number for that?

Note1: the applied code ia ASME VIII Div II

Note2: If the substitute NDT is UT with permanent record but also it's difficult to get it what is substitute to get NDT with permanent record????

 

Eng/Mostafa Kamel

Senior Welding Engineer

SIEMENS

+20104410009


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...