Skip to main content

[MW:811] [MW:810]] Bolt coating.


In addition to Raghu's email, sorry that I forgot to mention that the multilayer polymer coated bolts are being recommended for service temperatures of less than 200 deg.c and for all material bolting assemblies in highly corrosive atmospheric seashore site locations.

Just to pointout, additionally the zinc reacting with SS being refered as the LME-Liquid Metal Embrittlement effect. Which is true for metal coated SS bolting and painting material having zinc as an ingredient which can possible spill over during site painting acitivity and during fabrication or erection welds crossing the melting temp. of zinc which will lead to LME. Accidents of failure of massive pressure equipments have occured due to this minor mistake of paint spray on SS vessels before going for heat treatment in shops. Moreover this embrittlement move across the thickness.

With regards,
Kannan.




"Bathula Raghuram \(Mumbai - PIPING\)" <R.Bathula@ticb.com>
Sent by: materials-welding@googlegroups.com

29/05/2008 05:37

Please respond to
materials-welding@googlegroups.com

To
<materials-welding@googlegroups.com>, <piping_valves@yahoogroups.com>
cc
Subject
[MW:810] RE: 809] Bolt coating.





Zinc- or cadmium-coated steel fasteners shall not be used for applications above 400°F: these coatings may cause hydrogen embrittlement. Especially avoid mixing zinc- and cadmium-coated nuts, bolts, or washers at temperatures above 300°F: the zinc and cadmium will melt and mix. The resulting mixture is known to cause intergranular cracking, with subsequent failure of the fasteners in a short time. Failure of fasteners as described above can result in serious injury to personnel and damage to equipment. Cadmium or zinc is not permitted where it would be in contact with fuel oil, lubricating oil, grease, or petroleum-based hydraulic fluid. This restriction does not prohibit the use of cadmium or zinc plated fasteners in locations that are external to these systems if there is no danger of contaminating the working fluid. For example, cadmium or zinc plated fasteners could be safely used as hold down or mounting bolts for a hydraulic control valve since there is no danger of contact between the external fasteners and the fluid inside the valve. Personnel should wash their hands after handling cadmium plated fasteners to avoid ingesting cadmium.



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannan.Sundaram@Linde-LE.com
Sent:
Wednesday, May 28, 2008 9:41 PM
To:
piping_valves@yahoogroups.com
Cc:
materials-welding@googlegroups.com
Subject:
[MW:809] Bolt coating.

 

Felt to caution people who prescribe the bolt coating.


In an inhouse test of Polymer coated bolt of of a reputed Japanese vendor, which was to perform 4000 hours of salt spray test as per B 117, did not meet the requirement though the vendor's test certificates prooved so. The inhouse test was performed as in one of the plant it was used and has peeled off while normal wrenching and never stood even 1/4 of the life period gauranteed by the supplier. Literally all bolting of the plant had to be replaced by the client.


The final recommendation is that it is ideal to have a phosphating coat and a galvanizing or zinc coat and the final coat to be fluorocarbon polymer coat which really stood well in acc. with B117 in the inhouse test and has been proven in few operational plants.


So as a caution note, it would be a good practice to go for multiple coat rather than single coat for the general call for such coating requirements.


I do not want to name the companies explicity in this list for obvious reason.


Readers' experienced views are welcome.


With regards,
Kannan.
<br



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...