Skip to main content

Re: [MW:35988] P5A to P8

What about qw-423, it mention we can use alternative material for wqt,pls clear the doubt

Thanks&regards

Aslam khan
Mob:+965 66744128




On Tue, 3 Feb 2026 at 2:46 PM sridhar cn <sridharcn305@gmail.com> wrote:

As per ASME Section IX, welder qualification for a dissimilar weld (P5A → P8) performed using F-No. 43 filler cannot be done on 

P5A → P5A materials alone. The test coupon must include at least one P8 base metal to represent the metallurgical condition of 

the production weld. Therefore WQT must be performed on a CS + SS test coupon. CS + CS coupon with F43 is not acceptable under

ASME IX.

Sridhar.


On Tue, 3 Feb 2026 at 13:20, Aslam Khan <akchillu@gmail.com> wrote:
I have scenario in site, we have to qualify welders for cs to ss,but we dont have ss material available ,can we do with cs alone using f43 filler wire. wps- p5a to p8- f.no-43
Wqt - p5a to p5a- f.no-43

Thanks&regards

Aslam 


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAA7Erp%3DnRb20byLE0w2M14GDcFF3G1wkuy-5FzsTxyCpp7Q0Tw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYii0p7DJTBeeOVB9zdjhWGu%3DpVtVLzmVxXP6tXB02rmZWw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAA7ErpnqCZv8bLpw0GHh%3D-ifZnkKCJ7jBvK_kpe3xVPBQD-C_Q%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .