Re: [MW:33190] RE: PWHT Segment Wise for 9 Meter Dia Vessel

Dear Jayakumar
Not exactly. UW 4-(a)(8) covers everything else. As i mentioned it is not a preferable/recommended method (either go with Modular or Internal firing are most appropriate). 

"provided that other measures (based upon sufficiently similar, documented experience or evaluation) are taken that consider the effect of thermal gradients,
all significant structural discontinuities (such as nozzles, attachments, head to shell junctures), and any mechanical loads which may be present during PWHT.
The portion of the vessel or component outside the soak band shall be protected so that the temperature gradient is not harmful".


On Sun, 26 Jun 2022 at 11:55, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Raghuram,

Just for knowledge purpose. Do ASME Sec.VIII Div.I the applicable code permit LOCAL PWHT of Longitudinal seams.



Thanks & Regards

J.Gerald Jayakumar




On Sunday, 26 June, 2022 at 07:46:29 am GMT+4, Raghuram Bathula <raghurambathula@gmail.com> wrote:


Although no restriction in code preferable methoud could custom build modular furnace (with panel construction) at site

It is straight forward method for cir seams, however for long seams you have to work a methodology for placing coils locally using WRC 452 guidelines, probably  supplimented with an FEA to check thermal stresses

On Sat, Jun 25, 2022, 8:21 PM <pgoswami@rogers.com> wrote:

Hi,

It's allowed by Sec VIII, DIV1. Please see the highlighted clauses as below.

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

UW-40 PROCEDURES FOR POSTWELD HEAT TREATMENT:

From: vishal hirde <vishalhirde1988@gmail.com>
Sent: June 25, 2022 8:24 AM
To: materials-welding@googlegroups.com
Subject: PWHT Segment Wise for 9 Meter Dia Vessel

 

Dear All,

 

We are fabricating a Vessel of Diameter 9 Meter at Site, requires PWHT: Material Grade SA 516 Gr. 70.

 

 For Circumferential Joint PWHT can it be performed Segment Wise as diameter is more??

 

Pl. Confirm as per ASME Sec VIII Div 1 can it be done in Segment Wise. 

 

--

With Best Regards,

Vishal Hirde




---

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVubnaK4qDatj9JENMwNGPw7AZOFa%2BcCg4r9HrRPYDqc86Ew%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...