Wednesday, August 19, 2020

Re: [MW:31339] Re: Impact test requirements for LAS

As per  ASME B 31.3, LAS are exempted for impact test till -29 deg c  irrespective of thickness.

Regards
Atul Khatri

On Wed, Aug 19, 2020 at 9:58 AM Paidi <bobsuresh24@gmail.com> wrote:
Well said... Exactly.. Coarse grained steel does not required Imoact test requirements unless until service is different than normal... Cryogenic and all 

On Wed, 19 Aug 2020, 09:39 Customer Care, <bricenori@hotmail.com> wrote:

Dear Kiran,

 

It is rare that a low Cr-Mo alloy steel such as Group P5B is required to have an impact test at -29 C in its weld.

These steels are resistant to high temperatures of approximately 470 C to 650 C. So for what impact test? Structurally, for high temperature service a steel with a coarse grain size ASTM 4-5 (creep and oxidation resistant) is needed; and for low temperatures, tough steels with fine grain structure ASTM 8-9 are needed, which are suitable for cold service> -29 C to -45C.

 

The steels grouped in P5B are coarse-grained.

 

ASME B31.3 does not call for impact test at this temperature -29C. First of all, Kiran you must check the service temperature range of this pipe and its welding. What is approved in the Customer's specifications? I think your Customer  is wrong. Talk to him.

 

Regards,

 

Ramon Briceno/ Corrosion-Materials & Welding Engineer

 

Sent from Mail for Windows 10

 

From:
Sent: Tuesday, August 18, 2020 3:36 AM
To: Materials & Welding
Subject: [MW:31328] Re: Impact test requirements for LAS

 

Dear Experts,

 

Please I need your answer to my above query. 

 

My client has mentioned the above 25 mm Impact test would be required, in accordance with B31.3.

 

Question: Are materials, for which a temperature of −20°F (−29°C) is listed in the Minimum Temperature column of

Table A-1, exempt from impact testing for any combination of thickness and temperature above −20°F (−29°C)? Reply: Yes.

The minimum temperature in our scope is not below minus 29°C. If B31.3 calls for impact test within this temperature.

 

Your feedback is very important to me.

 

 

On Tuesday, July 28, 2020 at 10:12:01 AM UTC+5:30 K K wrote:

Dear Experts,

 

Please look into my query, please give me your response on my doubt.

 

Thanks

 Kiran 



On Monday, July 27, 2020 at 11:29:05 AM UTC+5:30, K K wrote:

Hi Experts,

 

"Good Morning"

 

My query has below.

 

Help me to prepare pWPS.

Process : GTAW +SMAW

Material : P.No - 5B   

ASTM A335 Grade P9.
Pipe Size - 16" Sch-60.
Thickness: 16.66 mm
Thickness range: 5mm to 33.32 mm
According to ASME B31.3 Table 323.3.1 shall I required an Impact for the above-mentioned thickness and material.
As per my knowledge, the above 25 mm impact test would be required. 
How I can find according to line class where impact test required or not.
If a minus 29° C impact test not required for LAS. 

When we shall consider the impact test exemption. 

 

And regarding consumable for P No- 5A 

ASTM A335 Grade P22

 

if I use ER90S-B3 ok or shall I use ER80S-B3 because my client suggest me to use ER80S-B3 please clarify way?

 

Thanks in advance 

 

Regards

Kiran

 

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e850f3f0-ffab-4097-b05e-5e8063cc163fn%40googlegroups.com.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BL0PR03MB4243D86E83ED1D6C00059921AA5C0%40BL0PR03MB4243.namprd03.prod.outlook.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAA%3D1_-xrRM5VdAO1EZe4LPiXQENTG0i0qv3d_ooFsqbGVW%3DM%2BA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACKOSeB9LNhoe9Zxf2T2AHAMq0w4KL4jpC7aNBPPSfdgyVK47Q%40mail.gmail.com.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...