Dear experts,
We have carried out FCAW WPQR with PWHT. Welding consumable is E71 T12 CJ. Below are the conditions
Test coupon thk- 70 mm
Parent material- S355 G8+N
Process- FcAW
Welding consumable- E71T-12CJ
PWHT Temp- 580 deg C
Soaking time - 280 minutes
Impact test temp- minus 40 deg C
Heat input range (root)- 1.0-1.6 KJ/mm
Heat input range (cap)- 1.0-1.4 KJ/mm
Thermal efficiency- 0.8
Welding position-3G
The above welding consumable is recommended for PWHT.
The impact values are too low at root as well as cap.
Energy values- 16,15,25 J (root)
Energy values- 30,30,31 J (cap)
Can you please focus on impact values failure reasons?
Even if keeping low heat inputs the test has failed.
What could be the possible reasons of failure?
And with the same conditions WPQR passed with 2G position.
Please focus on possible reasons.
Regards,
Vishal
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f1bead3a-d789-461c-a010-2e501ebb1e19%40googlegroups.com.
Subscribe to:
Post Comments (Atom)
[MW:35668] Selection of Filler/Electrode.
Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment