Re: [MW:28445] WELDING P11 WITH P91 STEEL

Weld p22 and P91 (Pup piece) and SR. Then join p11 with p22. 

On Fri, 19 Oct 2018 4:27 pm DDN VERMA, <vermananhu@gmail.com> wrote:
Dear Sirs,

I read several methods to join a P11 [1.25 Cr- 1/2 Mo] pipe to P91 [9Cr - 1 Mo] pipe, such as :

1. Weld using filler metal corresponding to corresponding to [2-1/4Cr - 1Mo] steel & post weld heat treat at appropriate temp..

2. Butter P91 with  filler corresponding to  [2-1/4Cr - 1Mo], post weld heat treat & weld with P11 & re-post weld heat treat it.

3. Use a P22 pup piece to join P11 with P91, etc. etc.....  

However, I wish to know, which is the most appropriate method taking into considerations the overall weld-integrity and high temperature strength of the weldment.

Please help to clarify my doubts.

THANKS,
DDN VERMA

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...