Re: [MW:23366] QW 200.4(b) - Combing two PQRs // SA516 Gr.70N + UNS N 08825. ( 40+3 mm) // closing seam

Are you sure of your consumable selection?

On 30 August 2015 at 11:00, Dhamodaran <dhamurocksu@gmail.com> wrote:

Dear All,

pls. go through the below scenario and provide your feed backs.


thanks.

Job Details : -

 

1.       Material               :               SA516 Gr.70N + UNS N 08825. ( 40+3 mm)

2.       PWHT                    :               Yes

3.       Impact                  :               Not required

4.       Vessel Size          :               ID-910 mm ; TL to TL -2000 mm

5.       Opening size      :               6"

6.       Overlay welding is for corrosion resistance only. Not considered in design thickness.

 

Background  : Since there is no accessibility to do the overlay welding on closing Circ seam (Cat – b). So I have to include the clad thickness in the butt joint. I.e ( 5-6 mm GTAW root with ER NICrMo-3 & Rest with SAW EM12K)



Query : I have two PQR as below mentioned, Can I combine both PQR to do the above butt welding?

 

PQR 1 :-

1.       Material               :               SA 516 Gr.70 + UNS N 08825 TO SA 516 Gr.70 + UNS N 08825 

2.       Thk                      :               13 + 3 mm

3.       Process                :               GTAW

4.       Consumable      :               ER NiCrMo – 3 (F – 43)

5.       PWHT                    :               Yes.

 

PQR 2 :-

1.       Material               :               SA 516 Gr.70N TO SA 516 Gr.70

2.       Thk                         :               38 mm

3.       Process                :               SAW

4.       Consumable       :               EM12K (F – 6)

5.       PWHT                    :               Yes.



--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVubmuKQJbQ8tKNjbOFu_2vndGZHBpoDoTMAUscZw2vv7Cew%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...