Hi!
In addition to improper use of Wire brush,Excessive grinding caused the removal of Cr Oxide film and after that Improper Pickling and passivation causes such type of rusted surface
Regards
Hegde Prakash
--------------------------------------------
On Sun, 26/10/14, Vino Varghese <vinopvarghese@gmail.com> wrote:
Subject: Re: [MW:22173] Rust on Stainless Steel Weld Joints
To: materials-welding@googlegroups.com
Date: Sunday, 26 October, 2014, 8:27 PM
Hi!!
Most probably the wire brush/grinding wheel
(Carbon Steel) would have played the culprit.
Please check that SS wire brush of good quality
has been used.
RegardsVino
On Sat, Oct 25, 2014
at 10:55 PM, Weaver, mark <Mark.Weaver@honeywell.com>
wrote:
Incorrect filler metal or contaminated brush/grinding
discs. PMI the weld metal to determine metallurgy.
Sent from my iPhone
On Oct 25, 2014, at 10:51 AM, "Sahavas v s" <sahavas143r@gmail.com>
wrote:
Hi,
It has been observed on all weld joints were corroded with
rust, but components dont have any rust. can any one answer
me the reason why weld joints have only corrosion not on
base metal?
Pipe : A312 TP 316 L
Filler wire : ER316L
Weld Type : Butt weld
--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
---
You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails
from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
---
You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
---
You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment