Re: [MW:22157] IQI-1A and IQI-1B

Dear Mohamed,

The Asme section V article T-276.2 (a) The thk on which IQI is based is the nominal single wall thickness + applicable estimated weld reinforcement not to exceed the maximum permitted by design code applicable.The actual measurement of the weld reinforcement is not required.

Now in your case thk 5.54 + 1.6 mm(check) = 7.14 mm.If you refer table T-276, correspondence wire type essential wire is 6 source side and film side essential wire is 5.

As per table T- 233.2 Set A & B both having common wire no 6. For DWDI pipe only source side placement of IQI allowed.

As long as if used Set B IQI and visible wire is 6 th one then required  sensitivity is achieved. Acceptable if source side IQI used. Both IQI can be used Set A and Set B if required 6th wire source side visible and set A for film side.

Sensitivity is based on essential wire not on IQI Type as per table 276.

Please check the applicable design code ASME 31.3 and Sec Viii for applicable reinforcement for the thickness .

Regards
Shridev


On 19 October 2014 20:25, Murugesh Anna <anna.murugesh@gmail.com> wrote:
Dear All,

IQI 1A is correct.

On Sat, Oct 18, 2014 at 5:39 PM, S.Mohammed <mohd52100@gmail.com> wrote:

Dear all,

Pipe thk :5.49mm
Mat :CS

Iqi selected based on thickness+reinfor(2mm) we selected IQI 1B.but client insist to.use us IQI 1A and given reshoot for using IQI 1B.

Is it correct the give reshoot?

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Best Regards,
Anna.Murugesh.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...