Sunday, October 26, 2014

Re: [MW:22171] Rust on Stainless Steel Weld Joints

Hi
 
It can be due to mixup of filler wire during welding or use of incorrect grinding wheels.
 
You can carry out PMI test and check for free iron contamination by conducting Ferroxil test / Copper sulphate test. Refer ASTM A967 / ASTM A 380 for details.
 
Regards
 
Prem Nautiyal
B.Tech, MMM, IWE, CSWIP 3.1, ASNT NDT Level III.
cell: 9769316004
Mumbai.
 


On Sunday, October 26, 2014 8:50 AM, "Weaver, mark" <Mark.Weaver@honeywell.com> wrote:


Incorrect filler metal or contaminated brush/grinding discs. PMI the weld metal to determine metallurgy. 

Sent from my iPhone

On Oct 25, 2014, at 10:51 AM, "Sahavas v s" <sahavas143r@gmail.com> wrote:

Hi,

It has been observed on all weld joints were corroded with rust, but components dont have any rust. can any one answer me the reason why weld joints have only corrosion not on base metal?

Pipe : A312 TP 316 L
Filler wire : ER316L
Weld Type : Butt weld
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...