Mr. Ahmed Osman,

Surprise.... you don't know the material and you advised to use E9018-D1.!!!!!!!!

Please do not do such things. Be clear about the material, electrodes and process to be used before attempting to do any welding( Please do welding procedure qualifications before welding). Let not there be any disasters because of this type of actions.... 

Dear all, as per my opinion, we should not comment on using electrode, temp etc.......as the material is not known and he already done an experiment. By luck..... the crack appeared...if not...... Let him find any stenciling/punch/description or any thing that have proper tracability to the actual material used.

Mr. Ahmed Osman, there are many specialists in this group who can support you. Please come with the proper material, they will support you to have a trouble free welding process. 


-- 
----------------------
Hareesh K V
+91-9447625012



On Tue, Mar 26, 2013 at 11:32 AM, <jsrisud@gmail.com> wrote:
Dear Ahmed,

If you can't test the rail material for composition, atleast test with magnet.

Mostly, rails are made of Hadfield manganese steels which are non-magnetic.

If so, weld with AWS E 307 - 16 without any pre-heat on the rail part.

This is the best recommended solution for joining Hadfield steel to Carbon steel.

JS
Sent from BlackBerry® on Airtel

From: ansary sayed <ansary_77@hotmail.com>
Date: Mon, 25 Mar 2013 21:22:39 +0200
Subject: RE: [MW:17218] Welding Train Rail to CS base Plate

you should give the standard type written on the rail parts and search about that type material to know the electrode required.


          Eng\ Ansary
email:ansary_77@hotmail.com
Mobile :01283667723-01114206108

 

From: A.osman81@yahoo.ca
To: materials-welding@googlegroups.com
Subject: [MW:17213] Welding Train Rail to CS base Plate
Date: Mon, 25 Mar 2013 18:07:19 +0300

Dears

I face a problem in my site … I have a rail do not know its material … we need to weld this rail to CS base plate (fillet weld) .. I told them to use E9018-D1 but it was not available they use 7018-1 but joints is cracked … please confirm me the electrode to use

** the rail is from Turkish railways rails

Ahmed


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...