Dear Ahmed,

If you can't test the rail material for composition, atleast test with magnet.

Mostly, rails are made of Hadfield manganese steels which are non-magnetic.

If so, weld with AWS E 307 - 16 without any pre-heat on the rail part.

This is the best recommended solution for joining Hadfield steel to Carbon steel.

JS
Sent from BlackBerry® on Airtel

From: ansary sayed <ansary_77@hotmail.com>
Sender: materials-welding@googlegroups.com
Date: Mon, 25 Mar 2013 21:22:39 +0200
To: Group welding<materials-welding@googlegroups.com>
ReplyTo: materials-welding@googlegroups.com
Subject: RE: [MW:17218] Welding Train Rail to CS base Plate

you should give the standard type written on the rail parts and search about that type material to know the electrode required.


          Eng\ Ansary
email:ansary_77@hotmail.com
Mobile :01283667723-01114206108

 

From: A.osman81@yahoo.ca
To: materials-welding@googlegroups.com
Subject: [MW:17213] Welding Train Rail to CS base Plate
Date: Mon, 25 Mar 2013 18:07:19 +0300

Dears

I face a problem in my site … I have a rail do not know its material … we need to weld this rail to CS base plate (fillet weld) .. I told them to use E9018-D1 but it was not available they use 7018-1 but joints is cracked … please confirm me the electrode to use

** the rail is from Turkish railways rails

Ahmed


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...