Hi MPK
 
I would like to share one practical example from my past assignments.
In UT after SAW welding of CS, we were getting fine cracks.
The WPS was religiously followed and we were confused !
 
After lot of investigation we found out that our welding operator had made short the SAW nozzle during welding which had caused copper contamination in the weld and resulted in cracks.
 
Regards
 
Prem Nautiyal

Mobile     +91 9004063879 / 9769316004

 
 


--- On Wed, 11/30/11, pgoswami@sympatico.ca <pgoswami@sympatico.ca> wrote:

From: pgoswami@sympatico.ca <pgoswami@sympatico.ca>
Subject: RE: [MW:13103] what is the root cause for copper crack in saw welding ?
To: materials-welding@googlegroups.com
Date: Wednesday, November 30, 2011, 9:22 AM

 Hi MPK,
 
 
It's a form of solidification cracking caused  due to localized segregation of low melting elements. Copper is one of the elements which tends to form so, for C.S and high strength and medium strength low alloy steels.
 
Please see the reference below.
 
Thanks.
 
P.Goswami,P.Eng,IWE
 
http://content.lincolnelectric.com/pdfs/knowledge/articles/content/weldcracking.pdf
 

Date: Tue, 29 Nov 2011 16:32:37 +0300
Subject: [MW:13100] what is the root cause for copper crack in saw welding ?
From: ranmi2007@gmail.com
To: materials-welding@googlegroups.com

Dear Experts,
What is the Root cause for copper crack in SAW welding ?

thanks,
MPK


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...