Re: [MW:12264] If Dia of Filler Rod changes what would be Volts , Amps & Travel Speed

you have to maintain heat input,

as heat input = voltage * current / travel speed

regards

dinesh

On Thu, Aug 18, 2011 at 4:58 AM, Abraham <QIS-009@hdec.co.kr> wrote:

Dear all

 

I need to make a WPS as per ASME SEC IX & Construction Code is ASME B31.3

 

PQR :  12" 42 THK 

Material :  SA335 P22

Process :  GTAW + SMAW

 

Actual Filler Wire Used in PQR  : 3.2 mm  Dia Rod  ( Amps : 100 ~ 125  , Volts : 23 ~ 26 , Travel Speed : 10 ~ 15 Cm / Min )

 

But in our site we are using 2.4mmm , 3.2 mm , 4.0 mm Dia Filler Rods

 

I want to make a WPS mentioning Current , Volt  , Travel speed for this 2.4 mm & 4.0 mm Rod also .

 

What basis  and Which clause I can get consequent A , V & TS  ?  

 

 By below clause we can support our WPS but cant get the value for A , V & TS .

                                             

                                               (i) 404.3 Change in Size of Filler metal is Non Essential Variable

                                               (ii) 409.8 Change in I & E Range is an Non Essential Variable

                                               (iii ) 409.1  Heat input increase in Supplementary Essential Variable . My case no need Impact Testing

 

 

Thanks and Regards

 

A.P.Abraham ,

Qatar .

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...