Re: [MW:5811] MPI vs DPI

Amir,

in general fabrication of mild steel, there is no reason why DPI can not
be used. It is actually a common enough practice ( you would rarely walk
into any fabrication shop without seeing some cans lying around). I'm
assuming the purpose is just for a general overview of weld quality such
as fillet welds and not as a substitute for penetration butt welds. MPI
& DPI in this instance perform the same basic function, and that is the
detection of surface defects.

Don't get confused by claims that MPI can detect subsurface - it can -
but interpretation is difficult and also subjective. If you are looking
for subsurface defects you use Radiographic or ultrasonic testing.

hope this helps

Declan

On 30/06/2010 13:14, Amir Zakee Adnal wrote:
> Declan
> We are doing some fabrication on normal carbon steel but we don't have
> the MPI set at this moment. My client would like to have some NDT
> tested. I need to convince my client that DPI is good enough to get
> the fabrication tested.
>
> Regards,
> Amir Zakee
>
> On 6/30/10, Declan Foley<declan1foley@eircom.net> wrote:
>
>>
>> MPI is for ferromagnetic materials only. It is supposedly useful for
>> defects of depth 6mm, but ask anyone who performs the tests and they
>> will tell you it is not!
>>
>> DPI can be conducted on any material. It is not recommended on materials
>> that have porous surfaces such as castings and the like.
>>
>> Strictly speaking they are both considered surface tests. As regards
>> substituting one for the other, I have never come across any situation
>> where you couldn't. What are you testing?
>>
>> Declan
>>
>> On 29/06/2010 17:35, mohammed helal wrote:
>>
>>> The major difference is the DPI is only for the defects that open to
>>> the surface and the MPI for the subsurface defect ( 6 mm deep).
>>>
>>> Eng.MOHAMMED ABD EL-AZIM HILAL
>>> MECHANICAL ENGINEER
>>> CSWIP 3.1 - NDT (RT- MT - PT)
>>> OTISHAN CONSULTANT ENGINEER
>>> 00966-502612218 - 0020103124557
>>>
>>>
>>> --- On *Tue, 6/29/10, george.dilintas@gr.bureauveritas.com
>>> /<george.dilintas@gr.bureauveritas.com>/* wrote:
>>>
>>>
>>> From: george.dilintas@gr.bureauveritas.com
>>> <george.dilintas@gr.bureauveritas.com>
>>> Subject: Re: [MW:5791] MPI vs DPI
>>> To: "materials-welding"<materials-welding@googlegroups.com>
>>> Date: Tuesday, June 29, 2010, 7:06 PM
>>>
>>> Mpi can be used only on ferromagnetic materials
>>>
>>>
>>> ----- Original Message -----
>>> From: Amir Zakee Adnal [amirzakee@gmail.com
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=amirzakee@gmail.com>]
>>> Sent: 29/06/2010 16:52 ZE5
>>> To: materials-welding@googlegroups.com
>>>
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=materials-welding@googlegroups.com>
>>> Subject: [MW:5787] MPI vs DPI
>>>
>>>
>>>
>>> Dear all
>>> What is/are major difference between MPI and DPI? Can MPI be
>>> substitute with DPI? Is there any code or standard that allow such
>>> substitution?
>>>
>>> Regards,
>>> Amir Zakee
>>>
>>> --
>>> To post to this group, send email to
>>> materials-welding@googlegroups.com
>>>
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=materials-welding@googlegroups.com>
>>> To unsubscribe from this group, send email to
>>> materials-welding-unsubscribe@googlegroups.com
>>>
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=materials-welding-unsubscribe@googlegroups.com>
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel
>>> views and meant for educational purposes only, Users must take
>>> their own decisions w.r.t. applicable code/standard/contract
>>> documents.
>>>
>>> --
>>> To post to this group, send email to
>>> materials-welding@googlegroups.com
>>>
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=materials-welding@googlegroups.com>
>>> To unsubscribe from this group, send email to
>>> materials-welding-unsubscribe@googlegroups.com
>>>
>>> <http://us.mc1138.mail.yahoo.com/mc/compose?to=materials-welding-unsubscribe@googlegroups.com>
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel
>>> views and meant for educational purposes only, Users must take
>>> their own decisions w.r.t. applicable code/standard/contract
>>> documents.
>>>
>>>
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding-unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel views
>>> and meant for educational purposes only, Users must take their own
>>> decisions w.r.t. applicable code/standard/contract documents.
>>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding-unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...