Dear Mahmood,

The UNS number for SS 329 is UNS S32900. Refer to ASTM/ ASME A/SA240,
against grade 329.

This grade is one of the oldest DSS group which is having higher carbon
content ie. 0.08% compared to recent DSS, maximum of 0.03 to 0.04.

The recommended filler metal can be either E/ER2209 or E/ER2553. It is
suggested to use E/ER2553 at root and subsequent passes with E/ER2209.

As for as welding point of view, the heat input should be restricted to
1 to 1.5KJ/mm in order to avoid slow cooling.

Regards,

L. Prabhu kumar,

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Bathula
Raghuram (Mumbai - PIPING)
Sent: Thursday, March 25, 2010 1:48 PM
To: materials-welding@googlegroups.com
Subject: [MW:4606] RE: 4605] Welding consumable for SS 329

Pl specify UNS# or full specification, if it is for UNS# S32950/F52, you
may use E/ER 2209

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Mehmood Javed
Sent: Thursday, March 25, 2010 11:56 AM
To: materials-welding@googlegroups.com
Subject: [MW:4605] Welding consumable for SS 329


Dear All,

Can somebody let me know the welding consumable specifications for SS
329 forging,

Regards,

Mahmood

Filtered by Hosted Filtering


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.

To unsubscribe from this group, send email to
materials-welding+unsubscribegooglegroups.com or reply to this email
with the words "REMOVE ME" as the subject.


-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or

entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged

information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution

or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If

you have received this communication in error, please notify us immediately by responding to this email and then

delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete

transmission of the information contained in this communication nor for any delay in its receipt.
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

To unsubscribe from this group, send email to materials-welding+unsubscribegooglegroups.com or reply to this email with the words "REMOVE ME" as the subject.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...