Usually the material specification will require that a minimum  of 87.5% of the ordered nominal wall thickness be maintained. This can be verified by blending and baseline UT. One other requirement is the "workmanlike finish". This is a subjective judgement. In either case, if buildup is required, ensure that your organization is certified to repair fittings and perform welding in accordance with approved WPS.  


On 2010-01-21, at 2:09, daniel iordache <daniel.iordache@gmail.com> wrote:

Hello 
the better way about pitting analyze and to get a right decision is to contact a corrosion engineer to evaluate area according with visual and ultrasonic testing report- he will calculate base on remaining thickness, length, material spec, operation pressure, safety factor the corrosion allowance and the remaining strength of material for corroded subject (api 31G).....other is to calculate all above according API 579.....

regads





On Wed, Jan 20, 2010 at 11:45 PM, michael lawrence <michael@lawrence2227.fsworld.co.uk> wrote:
dear sir anything biger than the calaberation notch wich is 1mm is a defect and i do believe it would be down to the welding engineer to make a desision as to wether or not to use the elbow i do bilieve that there is no specific area as to how much pitting would b allowed the decision would be yes or no or can the pitting b eliminated i.e repair welded as a welding inspector i would have some idea as to wether or not it way be used but would hafto come from a engineer and depending on what product would be going through the material
 
 
regards
mike.
----- Original Message -----
Sent: Wednesday, January 20, 2010 9:52 AM
Subject: [MW:4105] Pitting acceptance criteria

Dear all,
 
We received one 40" elbow (ASME 16.9) ASTM A 860 material having so much pitting on full external surface. Which standard we can refer for the acceptance criteria? 
 
 
I referred in ASTM A 860, its talks about only depth of surface discontinuity(5% of the nominal thickness),  there is no detail about the area of the pitting allowance.
 
Please help me on this issue. Very urgent
 
Regards,
 
Gulam Kader 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



No virus found in this incoming message.
Checked by AVG - www.avg.com
Version: 8.5.432 / Virus Database: 270.14.151/2633 - Release Date: 01/19/10 17:49:00




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--
Daniel Iordache
Bureau Veritas - Angola
Mechanical& Welding Surveyor
Mobile Ao: +244921544583
Mobile Ro:   +40721731728
E-Mail: daniel.iordache@gmail.com
          daniel_iordache@yahoo.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...