Hi Prem,

 

Could you be more specific about your query:-

 

·    Underclad Cracking Test— is it related to SAW strip cladding of S.S / Inconel on Reactor Pressure Vessels (RPV) shells. What kind of reheat cracking tests you have to do? Usually reheat cracking is very difficult to simulate.

 

·    Regarding hydrogen cracking, there are standard tests developed and adopted by the industry. If you are familiar with Tekken Y-Grove test, it's a very popular test for hydrogen cracking. What's the test you're asked to perform in this case.

 

However underclad  hydrogen cracking  is a bit different issue. Typically it's commonly performed  as autoclave testing, and ASTM –G-146, is the standard followed for this underclad hydrogen disbanding test.

 

Due to copyright issue, I can not post the ASTM standard. However the attached article tells clearly how this test is performed.

 

Thanks

 

Pradip Goswami,P.Eng

Senior Engineer/Specialist(Welding-Metallurgy)

Engineering & Training Services Division

ONTARIO POWER GENERATION Inc.

PO Box-2000, RR-55(South)

Nanticoke, Ontario,N0A1L0

Tel:-(519) 587-2201, Ext 3107--in Nanticoke

         (416) 231-4111, Ext 5925--in Kipling,Toronto

Fax: (519) 587-6814

Email-pradip.goswami@opg.com.

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PREM SHANKARDUTT NAUTIYAL
Sent:
Wednesday, January 27, 2010 1:20 PM
To: materials-welding@googlegroups.com
Subject: *****SPAM***** [MW:4160] Underclad cracking tests

 

Dear All

Can anyone provide some article / explanation / detailed procedure about how to prepare specimens and conduct test for the following Underclad cracking test ---


1)Weld specimen for reheat cracking.
2)weld specimen for Hydrogen induced cracking.


The job is a PV, code of construction is ASME Sec
III, NB.

Regards

Prem Nautiyal

PREM S NAUTIYAL
CELL : 9820313278

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...