[MW:35596] Re: Welding Consumable Selection for the API Materials

Considering that you are welding long/ helical seam of pipe

1. API 5L Gr. B + API 5L Gr. B = 
Seam Weld: GMAW Tack: ER70S6, SAW ID and OD EM12k + Flux,  Repair SMAW 6018
2. API 5L Gr X52 + API 5L Gr X52 = 
Seam Weld: GMAW Tack: ER70S6, SAW ID and OD EM12k/EA2 + Flux, Repair SMAW 7018
3. API 5L Gr X70 + API 5L Gr X70 = 
Seam Weld: GMAW Tack: ER70S6, SAW ID and OD EA2 + Flux,  Repair SMAW 8018

Saw wire selection will also depends upon CVN requirements.
Regards
Punit Dubey
On Friday, May 2, 2025 at 11:03:06 AM UTC+5:30 Shivasankar A wrote:
Dear Friends,

Can you suggest me the Welding consumable ( Both Filler Wire & Electrode) for Below materials,  

1. API 5L Gr. B + API 5L Gr. B =
2. API 5L Gr X52 + API 5L Gr X52 = 
3. API 5L Gr X70 + API 5L Gr X70 = 

If any body having the WPS & PQR in the above materials. kindly share me for reference. These are the new materials for me. So Kindly help me guys.

Regards,
A.Shivasankar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/eb8ccfb3-146e-4482-afee-dd01190fa0ecn%40googlegroups.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...