Use NiCr3 or NiCrCoMo1.  (Inconel 625 Will be subjected to second hardening effect when it is exposed at this tem for longer periods. )

On Tue, 21 Jan 2025, 20:14 PARAI Reaction Channel, <saravanshyla@gmail.com> wrote:
Dear Sirs,

Please confirm the following weld details for my below 2 queries.

We have a tube to tube welding , in which the material is SB407 UNS N08810 ( P No. 45 ) and the design temperature is about 800 Deg C.

1) Can we use either ERNiCr3 GTAW weld rod Or ERNiCrMo-3 considering the above design temperature for UNS N08810, without having metallurgy issues , cracking etc?

Or which is the best suitable AWS class GTAW rod to withstand 800 Deg C for this weld?

2) To weld dissimilar materials , that is SB407 UNS N08810 ( P No. 45 ) to A312 TP 321H ( P No. 8 ), can we use ERNiCrMo-3 for a design temperature about 800 Deg C ?

Please give me some advice.

Best regards,
Saravanan Sornam,
Ansan-si,
S.Korea

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALV1rk%2BPQwLp189j%2B8eaB%2Bf%3Dasw0D-iqhzaQ4qq1M0AVTd8Ovg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eM7itbRs83TZBBfVFQEhWLxXZigkxeX0SZzfirkpzSxug%40mail.gmail.com.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...