dear expert

I have to do WPS and PQR details given below

 

Test coupon

Thickness -50 mm

Material - IS 2062 E 350 C 

Code - ASME 

Position - 3G

Process - SMAW 

Electrode - E-7018

Impact = -20C @ 27J

Stress Relieving - 605+/- 10c

Rate of heating/cooling- 100c/hr.

 

Whether if Rate of heating / cooling is 100c/hrs will it affect the test result both UTS and Impact properties? : No, It's the Exposure time at the PWHT Temperature which matters most towards the UTS & Charpy Impact values. As a matter of fact, there is no need to maintain a cooling rate of 1000C/hr. You may increase the cooling rate to 150Deg C /hr or more.

 

As per UCS 56 ASME SEC 8 div 1 Max rate of heating and cooling 222c/hrs divided by max.metal thickness.

 

As my client need Rate of heating and cooling 100c/hrs.

 

Plz kindly clarify.

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOp_kKjwT0i_sWcf03H7PGvTrz0nXEFEmAmLKTsnX1y6Wwgzjg%40mail.gmail.com.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...