Well! the reason behind E3016L -15 recommendation is :
SMAW = E306L -  15 - It has lower  FN and in turn  better Notch Toughness values at -196   Deg C .
- 15 covering produce much cleaner weld metal( lesser Oxygen , Nitrogen) that is must for  achieving Notch Toughness values at -196   Deg C .


On Tue, Dec 22, 2020 at 9:11 AM sela <mechselastine@gmail.com> wrote:
Experts

Below  requirement given in one LNG project... 

Welding Consumables:
1. SMAW Consumables for Type 304L Stainless Steel Impact Tested at -196°C (-320°F).
Consumable:
ASME Specification SFA 5.4 in Part C, Section II Material Specification
- AWS Classification E316L-15
Certification and Testing:
ASME Specification SFA 5.01 in Part C, Section II Material Specification
- Lot Classification - C5
- Level of testing - Schedule K
Testing Requirements for each Lot of electrode:
Each Lot of electrode shall be certified with the minimum following testing:
- Chemical analysis of weld metal to meet the requirements for classification E316L
except the maximum phosphorus shall be 0.03% and the maximum sulphur shall be
0.02%.
- Delta ferrite determination per paragraph A6.9 of SFA 5.4. The weld metal shall be
a maximum Ferrite Number of 2 FN.
- Charpy V-notch impact test shall be performed on the weld metal in accordance
with SFA 5.4, paragraph A9.3.1. The weld test assembly shall be prepared and
welded with CVN specimens removed as per paragraph A9.3.5 of SFA 5.4. Five
impact specimens shall be tested at -196°C (-320F). The lowest and highest values
obtained shall be disregarded. The three remaining values shall be equal to, or
exceed, 20 mils of lateral expansion. The energy in ft-lbs and the percent ductile
fracture areas shall be reported for information.

Question
1) what is the technical  Reason behind for E316L -15 for Type 304L SS welding  SMAW process -cryogenic , however for GTAW process ER308L specified for Type 304L welding.  

Regards
sudhakar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6bfc38f9-dbf8-45be-8824-c954b3dec788n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3P8RiWD4rHFdynUbnebC5Uaiu8XWS97p91JYb0jNQcS0A%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...