Dear Sir,

Really Heat affected zone is measured regarding the micro-structure changes in the weld and also according to the experts. The theoretically calculation of HAZ may be not accurate to depend.
You can find such formula in chapter three of AWS Welding Handbook {Heat Flow in Welding}
1/Tp-To = 4.13pchY/ Hnet + 1/Tm-To;
where,
Y is width of HAZ in mm
h: plate thickness in mm
Tp is peak temperature,
To is initial plate temp (room temp or preheat temp),
pc-volumetric specific heat (J/mm3.C),
Tm is melting temp;
Hnet: net heat input (J/mm)

Regards,
Ankit Patel
Mo No : +91 8140255303

On Sun 6 Dec, 2020, 7:32 PM Hany Nabil, <eng.hanynabil20@gmail.com> wrote:
Dear exports,

For HAZ in side welding depending on heat input.
How to calculate HAZ distance ?
Any equation formula ?

Thanks,
--


 Best Regards,

 Eng. Hany Nabil
 Senior Welding Engineer
 Petrofac
 Engineering and Production Service
 Egypt Mobile: 002-01225622022




This message, including any attachments, may contain confidential and privileged information for the sole use of the intended recipient(s). Review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient, or authorised to receive information on behalf of the recipient, please contact the sender by reply email, and delete all copies of this message. While we have taken reasonable precautions to ensure that this message and any attachments are free from viruses, we cannot guarantee that they are virus free and accept no liability for any damage caused by this message or any attachments. Messages sent or received through our networks may be monitored to ensure compliance with the law, regulation and/or our policies.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP1YJmQSgbkHQ0wm56Errx%3Dab4xHVeHwh35oOGEVMeBpDPLhrA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALR-PuztSiN3LQ%2B8RQSE75oJkt3WhWzufr3gnLVoL5Mp3uQsdQ%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...