let us take the some essential variables one by one:
Pno: see QW 403.11 and then QW 424. The combination you have does not help. It qualifies only PNo 5B to Pno *.
A no: due to the dilution between a low alloy and stainless steel most probably it will not match.

So no chance, you need a new PQR

2016-11-17 15:31 GMT+02:00 Manoj John <manojacgnr@gmail.com>:
Dear Experts,

We have the following WPS as per ASME Sec. IX

Base metal - P5B + P8  (6" Sch 40 Pipe)
Welding process -  GTAW
Filler metal -  ER NiCr-3
Preheat temp - 180 degree C
PWHT - Nil
Trailing & backing gas -  Yes (Argon)

Can i use the above procedure for welding of ;

P5B group material fillet welding (seal welding of threaded joints) with ER NiCr-3 or ER NICrMo-3 GTAW process without PWHT 
Hardness test required for HAZ 235HV10.

your expert advice highly appreciated.

Thanks & Regards,
Manoj.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACgUO5nE%3DtZ-gmMz2cg%3DzBTMjGpOTCxSxUQwT7jSRDWn3SkFXw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40COijWh34HQ%2BUpz9xGvvrimST%3D3EO38Gh58dO-tp4hvXA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...