Re: [MW:23271] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)

Quote "NOTE ONE SHOULD NOT WELD ON AUSTENITIC  ALLOYS, WITH FERRITIC ELECTRODES. Just check the composition from  the basic rules of dilutions The reverse (using austenitic electrode on ferric steel)will work."Unquote.
The reverse also may not work (low FN and hot cracking). Superaustenitic filler metals like 309 are to be used in that case

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


"'Zeghanu Gigi' via Materials & Welding" ---11/05/2015 11:14:17---Dear Goswami,  As per your last message"   If you buttering with Inconel-182, thereafter welding  wi

From: "'Zeghanu Gigi' via Materials & Welding" <materials-welding@googlegroups.com>
To: materials-welding@googlegroups.com
Date: 11/05/2015 11:14
Subject: Re: [MW:23263] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)
Sent by: materials-welding@googlegroups.com





Dear Goswami,

As per your last message"   If you buttering with Inconel-182, thereafter welding  with B9 and B3 welding electrode, it'll create nothing but complex welding
metallurgy. NOTE ONE SHOULD NOT WELD ON AUSTENITIC  ALLOYS, WITH FERRITIC ELECTRODES. Just check the composition from  the basic rules of dilutions The reverse (using austenitic electrode on ferric steel)will work."

Are you so kind to be give us more details regarding " compex welding mettalurgy "created if buttering with Inconel 182 is followed by welding with B9 and B3 welding electrode.

Regards

GIGI ZEGHEANU

Welding Engineer

--------------------------------------------
On Mon, 11/5/15, pgoswami <pgoswami@quickclic.net> wrote:

Subject: [MW:23261] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)
To: materials-welding@googlegroups.com
Cc: rushabhpanjabi@gmail.com
Date: Monday, 11 May, 2015, 3:36



 
 

Hi
Rusabh,
 
There's
something wrong in the selection procedure of
welding electrodes. What you mentioned, i.e. use of Inconel
welding electrodes
applies for DMW between Grade-91 and Austenitic
S.S. 
 
If you buttering
with Inconel-182, thereafter welding
with B9 and B3 welding electrode, it'll create nothing
but complex welding
metallurgy. NOTE ONE SHOULD NOT
WELD ON AUSTENITIC
ALLOYS, WITH FERRITIC ELECTRODES. Just check the
composition from
the basic rules of dilutions. The reverse (using austenitic
electrode on ferric
steel) will  work.
 
This welding could
be easily done by using B3 or B9
welding electrodes , and  butt welding P22 to P-91
steel.
 
Thanks
 
 
Pradip
Goswami, P.Eng,IWE
Welding &
Metallurgical Engineer/Specialist
Ontario,
Canada
pgoswami@quickclic.net
pradip.goswami@gmail.com
 



From:
materials-welding@googlegroups.com
[
mailto:materials-welding@googlegroups.com] On Behalf Of
RUSHABH
PANJABI
Sent: Sunday, May 10, 2015 10:24 AM
To:
materials-welding@googlegroups.com
Subject: [MW:23260] Dissimilar
Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)



Hello,For dissimilar welding between P22 to
P91, i have used
Inconel  182 electrode.is it correct electrode.I have
also tried buttering
of inconel 182 on P22 and P91 and balance welding with B9
and B3.Then PWHT at
740 for 3  hours.. With buttering Side bend specimen
fails adjecent to
buttering in weld.. what can be reason for it?
--
You received this message because you are subscribed to the
Google
Groups "Materials & Welding" group.
To unsubscribe from this group and
stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To
post to this group, send email to materials-welding@googlegroups.com.
Visit
this group at
http://groups.google.com/group/materials-welding.
To
view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/ad0b14e6-b913-4190-8109-1362083f247e%40googlegroups.com.
For
more options, visit
https://groups.google.com/d/optout.



No virus found in this
message.
Checked by AVG -
www.avg.com
Version: 2015.0.5941 / Virus
Database: 4342/9741 - Release Date:
05/10/15



--

You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.

To post to this group, send email to materials-welding@googlegroups.com.

Visit this group at
http://groups.google.com/group/materials-welding.

To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/EA43582C738B425F9FDC017B5876299C%40homepg.

For more options, visit
https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/1431330483.18623.YahooMailBasic%40web171804.mail.ir2.yahoo.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...