Dear Goswami,
As per your last message" If you buttering with Inconel-182, thereafter welding with B9 and B3 welding electrode, it'll create nothing but complex welding
metallurgy. NOTE ONE SHOULD NOT WELD ON AUSTENITIC ALLOYS, WITH FERRITIC ELECTRODES. Just check the composition from the basic rules of dilutions The reverse (using austenitic electrode on ferric steel)will work."
Are you so kind to be give us more details regarding " compex welding mettalurgy "created if buttering with Inconel 182 is followed by welding with B9 and B3 welding electrode.
Regards
GIGI ZEGHEANU
Welding Engineer
--------------------------------------------
On Mon, 11/5/15, pgoswami <pgoswami@quickclic.net> wrote:
Subject: [MW:23261] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)
To: materials-welding@googlegroups.com
Cc: rushabhpanjabi@gmail.com
Date: Monday, 11 May, 2015, 3:36
Hi
Rusabh,
There's
something wrong in the selection procedure of
welding electrodes. What you mentioned, i.e. use of Inconel
welding electrodes
applies for DMW between Grade-91 and Austenitic
S.S.
If you buttering
with Inconel-182, thereafter welding
with B9 and B3 welding electrode, it'll create nothing
but complex welding
metallurgy. NOTE ONE SHOULD NOT
WELD ON AUSTENITIC
ALLOYS, WITH FERRITIC ELECTRODES. Just check the
composition from
the basic rules of dilutions. The reverse (using austenitic
electrode on ferric
steel) will work.
This welding could
be easily done by using B3 or B9
welding electrodes , and butt welding P22 to P-91
steel.
Thanks
Pradip
Goswami, P.Eng,IWE
Welding &
Metallurgical Engineer/Specialist
Ontario,
Canada
pgoswami@quickclic.net
pradip.goswami@gmail.com
From:
materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
RUSHABH
PANJABI
Sent: Sunday, May 10, 2015 10:24 AM
To:
materials-welding@googlegroups.com
Subject: [MW:23260] Dissimilar
Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)
Hello,For dissimilar welding between P22 to
P91, i have used
Inconel 182 electrode.is it correct electrode.I have
also tried buttering
of inconel 182 on P22 and P91 and balance welding with B9
and B3.Then PWHT at
740 for 3 hours.. With buttering Side bend specimen
fails adjecent to
buttering in weld.. what can be reason for it?
--
You received this message because you are subscribed to the
Google
Groups "Materials & Welding" group.
To unsubscribe from this group and
stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To
post to this group, send email to materials-welding@googlegroups.com.
Visit
this group at http://groups.google.com/group/materials-welding.
To
view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ad0b14e6-b913-4190-8109-1362083f247e%40googlegroups.com.
For
more options, visit https://groups.google.com/d/optout.
No virus found in this
message.
Checked by AVG - www.avg.com
Version: 2015.0.5941 / Virus
Database: 4342/9741 - Release Date:
05/10/15
--
You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/EA43582C738B425F9FDC017B5876299C%40homepg.
For more options, visit https://groups.google.com/d/optout.
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1431330483.18623.YahooMailBasic%40web171804.mail.ir2.yahoo.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment