There's something wrong in the selection procedure of welding electrodes. What you mentioned, i.e. use of Inconel welding electrodes applies for DMW between Grade-91 and Austenitic S.S. 
 
If you buttering with Inconel-182, thereafter welding with B9 and B3 welding electrode, it'll create nothing but complex welding metallurgy. NOTE ONE SHOULD NOT WELD ON AUSTENITIC ALLOYS, WITH FERRITIC ELECTRODES. Just check the composition from the basic rules of dilutions. The reverse (using austenitic electrode on ferric steel) will  work.
 
This welding could be easily done by using B3 or B9 welding electrodes , and  butt welding P22 to P-91 steel.
 
Thanks
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineer/Specialist
Ontario, Canada
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of RUSHABH PANJABI
Sent: Sunday, May 10, 2015 10:24 AM
To: materials-welding@googlegroups.com
Subject: [MW:23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)

Hello,For dissimilar welding between P22 to P91, i have used Inconel  182 electrode.is it correct electrode.I have also tried buttering of inconel 182 on P22 and P91 and balance welding with B9 and B3.Then PWHT at 740 for 3  hours.. With buttering Side bend specimen fails adjecent to buttering in weld.. what can be reason for it?

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ad0b14e6-b913-4190-8109-1362083f247e%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No virus found in this message.
Checked by AVG - www.avg.com
Version: 2015.0.5941 / Virus Database: 4342/9741 - Release Date: 05/10/15

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...