Thursday, November 27, 2014

Re: [MW:22379] AISI 4140 material

Dear Pravin,
Please follow the steps below.
1. preheat to 200 Deg. C
2. Use ER 80 S D2  for GTAW, if it is intended for root and hOt pass of a weld in a combination of processes, otherwise ER 100S D2.
3. Use E 10018 D2 or E11008 M for SMAW.
4. After welding put the blanket over the weld to allow slow cooling.
5. PWHT at 10 deg. lesser than Quenching temperature ( 630 Deg.C - 650 Deg.C) for atleast 2 Hours.
 
Thanks and Best Regards,
K.Rajagopal
 
On Wed, Nov 26, 2014 at 4:15 PM, Pravin Poornachandran <htcispravin@gmail.com> wrote:
Dear Expert,

Anyone have any experience welding on AISI 4140/4130 material?

What is the best welding consumable can be recommended for this kind of material.

Along my knowledge, 4140 is high tensile & high yield strength material which requires proper welding condition such as preheat, interpass temperature control etc.

Kindly assist me on the welding consumable for this kind for
SMAW
GTAW
FCAW/GMAW
SAW

Best regards,
Pravin Poornachandran
Singapore

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...