Re: [MW:22331] Super duplex ASTM G48 practice A & E

Dear Mr.Lalu,

Appreciate your explanation.

I have much better understanding now with the article which attached.

Best regards,
Pravin Poornachandran
Welding Engineer
Singapore

On Nov 22, 2014 3:07 PM, "LALU RAJENDRAN" <lalucpt@gmail.com> wrote:
Hi Mr. Pravin,

Method A is designed to determine the relative pitting resistance  of  stainless  steels  and  nickel-base,  chromium-
bearing alloys and Method B is the critical pitting temperature test for stainless steels. 

for super-duplex, you may consider the following factors 
1.ASTM G 48 Method A.
2. Exposure time shall be 24 hours.
3.Samples should not pickled or passivated before test as it may affect the test result.
4.Test temperature for UNS S32550, S32750, UNS S32760, S39274 weld samples (25% chromium "super" duplex)         shall be 40°C.

Examination and Evaluation: -No pitting at low-power magnification and maximum weight loss shall be less than 1.5 g/m2.

Please refer the attached article for further information

Thanks & Regards,

LALU R.P


On Fri, Nov 21, 2014 at 7:25 AM, Pravin Poornachandran <htcispravin@gmail.com> wrote:
Dear expert,

what is the different between practice A & E when comes to super duplex.
Normally which practice is widely used?

Kindly advice.

Best regards,
​​
Pravin Poornachandran
Welding Engineer
Singapore

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...