Skip to main content

RE: [MW:16837] Pitting Corrosion Resistance Failure in DSS

Mr.. Mani,

The intent of ASTM A 923, Method C.  is for detecting the presence of detrimental intermetallic phases in duplex stainless steels.  The acceptability criteria  for corrosion resistance is the by weight loss. The presence or absence of corrosion attack in this test is not necessarily a measure of the performance of the material in other corrosive environments; in particular, it does not provide a basis for predicting resistance to forms of corrosion not associated with the precipitation of intermetallic phases.

Various experimental results  have shown that , major intermetallic such as sigma phase 0.1-0.5% (volume  fraction) are easily tolerable by various duplex and super duplex S.S grades. However, when the volume percentage reaches a level of about 1% a detrimental influence is observed for both alloys. A percentage of σ-phase below 0.5% is perfectly acceptable provided pitting corrosion is the main concern.

From severity point of view this test is less severe than ASTM G-48A test.

Hence  for  application of  DSS for refining and petrochemical environments, this test is suggested by various codes, e.g API -938C. and NACE MR-103. Usually, if welded well with welding products of reputed manufacturers (e.g Metrode as mentioned) specimens should not fail.

What was the ferrite count and the volume fraction of intermetallics in the weld coupon??. Was it calculated ???

Appreciate your feedback.
 
Thanks.

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of E.S.Mani
Sent: Wednesday, February 20, 2013 4:30 AM
To: materials-welding@googlegroups.com
Cc: sivaselvam@kpoc.com.my
Subject: Re: [MW:16823] Pitting Corrosion Resistance Failure in DSS

 Dear Mr.Tariq,

Thanks for your info,

Yes the client spec was saying to do ASTM G 48 C.

Yes we used the PQR as per the consumable recommendation.

We used GTAW.

Dear siva,

Cold pass means second pass or next to the root pass.

Mani

On Wed, Feb 20, 2013 at 1:27 PM, Tariq Hussain <tariqhussain632@gmail.com> wrote:
Dear Mani,

1. Before planning for PQR, You have to confirm from Consumable Manufacturer that, Do they grantee their consumable to pass Corrosion test in accordance with ASTM 923 C, As most of Consumable Manufacturers prefer to test according to the ASTM G 48 Method (Which is actually standard for Pitting Corrosion Test, While ASTM 923 C is for Intergranular Corrosion Test).
2. Does your Project specification calls for Corrosion Test as per ASTM 923 Method C. If not, then go for ASTM G 48 C?
3. If ASTM 923 C is the requirement, then I shall suggest you to change Consumable Brand ( You may select Sandvik)
4. Which Welding Process, did you use?, If possible MIG can be useful, But there is no special restriction for using GTAW, SMAW or SAW. 
5. Conduct PQR Wedling according to all the recommendations of Consumable Manufacturer including those, shielding / purging gases & current ranges etc.
6. There is special technique with DSS & SDSS, depositing thick root pass and thin cold pass (as fast as welder can weld it).
7. Did you monitor Oxygen Level in Backing gas (if used) during welding, It should be less than 50ppm or according to Consumable manufacturer?

Regards

Tariq Hussain.



On Wed, Feb 20, 2013 at 6:08 AM, E.S.Mani <maniesbk@gmail.com> wrote:
Dear Experts,

We are welded DSS A790 UNS S31803 Pipe to pipe PQR welding and we sent it for Mechanical test. But we found PITTING.

The details are below and i attached the test result also.

Material                         :           A 790 UNS S31803 (Pipe to Pipe)

Size                              :           4" X 8.56mm

Filler Used                     :           ER2209 (Metrode) 2.4mm

Max. Interpass               :           Below 50ºC

Max. Heat Input             :           1.2 KJ/MM

Test Method                  :           ASTM 923 Methode C (22ºC – 24HRS)


Now we are planning to do the PQR again. So please give me you idea to avoid the failure again.


Thanks.



--

Regards,

E.Subramanian

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 



--

Regards,

E.Subramanian

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...