Dear sir
The selection of welding rod/ filler metal PREN . shall be littile
higher side that of parant material PREN, this will be give good
results,
Regards
GSR
On Wed, Feb 20, 2013 at 8:38 AM, E.S.Mani <maniesbk@gmail.com> wrote:
> Dear Experts,
>
> We are welded DSS A790 UNS S31803 Pipe to pipe PQR welding and we sent it
> for Mechanical test. But we found PITTING.
>
> The details are below and i attached the test result also.
>
> Material : A 790 UNS S31803 (Pipe to Pipe)
>
> Size : 4" X 8.56mm
>
> Filler Used : ER2209 (Metrode) 2.4mm
>
> Max. Interpass : Below 50ºC
>
> Max. Heat Input : 1.2 KJ/MM
>
> Test Method : ASTM 923 Methode C (22ºC – 24HRS)
>
>
> Now we are planning to do the PQR again. So please give me you idea to avoid
> the failure again.
>
>
> Thanks.
>
>
>
> --
>
> Regards,
>
> E.Subramanian
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment