Wednesday, October 28, 2009

[MW:3565] Re: 3559] CONSUMABLES

Dear Rajagopal,

I am also, requiring this procedure,i've got two failed PQR's
1)I tried to weld AISI4130 TO SA 182 F22V, with ER 80S-B2 & E8018-B2H4 It's failed in the WCL & Impact
Preheat: 260 Degree C Interpass:300 Degree C Maximum
PWHT:690 Degree , Heating & Cooling rate :150 Deg C/hr per inch thk
Holding time:90 minutes
Please advise do we have to follow mandatory appendix-31 for impact acceptance

2))I tried to weld AISI4130 TO SA 182 F22V, with ER 80S-D2 & E10018-D2 It's failed in the HAZ  & Impact @ -29 degree C
Preheat: 260 Degree C Interpass:300 Degree C Maximum
PWHT:675 Degree , Heating & Cooling rate :150 Deg C/hr per inch thk
Holding time:90 minutes

Please suggest me an other alternative consumable.I've to qualify this procedure urgently.Please anyone out there who can guide me in this

Thanks & Regards,
vipin george
Specialist services, Dubai

On Wed, Oct 28, 2009 at 12:12 PM, GERING, Erwin <Erwin.GERING@airliquide.com> wrote:

First idea is to use CrMo2 consumables (or CrMo1 could be solution too, depending on application / requirements)

Preheat 200 degrC

PWHT at 690 °C , however

·         PWHT temperature is depending on strength requirements 4130 and required charpy values in weld metal

·         duration is depending on wall thickness and required charpy values in weld metal

 

Stick electrodes

·         OERLIKON CROMOCORD 2 STC

·         OERLIKON OE KV3 HR

TIG rod:

·         OERLKON CARBOROD CrMo2  or

·         OERLIKON CARBOROD KV3 (=B2)

 

Erwin Gering

AIR LIQUIDE WELDING

OERLIKON_RVB_5cm.BMP

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens rajagopal kannan
Verzonden: woensdag 28 oktober 2009 8:23
Aan: materials-welding@googlegroups.com
Onderwerp: [MW:3559] CONSUMABLES

 

Dear Members,

Could you please suggest me the apt consumable for GTAW and SMAW to weld SA 182 Gr. F22 cl.1 with AISI 4130?

Thanks and Best Regards,

K.Rajagopal






--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

1 comment:

Anonymous said...

We recently ran a procedure welding F22 (mod 100Ksi) to F70 and used Tenecito 70 SMAW electrodes and PWHT at 630 DEgC Charpys and CTOD were ok

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...