[MW:978] RE: 974] RE: 971] RE: 970] Consumable For UNS31254 weldoverlay on SA516 Gr. 70

Dear All,
Just to add further to this,
Avesta P12-R Basic (ENiCrMo-12) is best suited for welding UNS S31254. The
Avesta P16 Basic electrode confirms to ENiCrMO-13 and is specifically
designed for welding 654SMO (UNS S32654) grades.

Regards,

Abby Joseph


-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram
(Mumbai - PIPING)
Sent: 28 July 2008 09:57
To: materials-welding@googlegroups.com
Subject: [MW:974] RE: 971] RE: 970] Consumable For UNS31254 weldoverlay on
SA516 Gr. 70


UNS31254 is similar to Type 254SMO of Avesta polarit; you may contact
them for their recommended combination (Avesta P16 or P12-R basic etc.)
ERNiCrMo-3 (AWS Specification A5.14) or ENiCrMo-3/ ENiCrMo-12 (AWS
Specification A5.11) can be used for depositing, depending on the
process you may choose. E309LMo also can be used for barrier layer.
Avestapolarit has 805 flux which can be used in case of SAW

Sandvik also got similar combination such as Sanicro60 etc...

For strip cladding Soudokay has got some combinations, such as
Soudotape625 with flux NFT201/EST201 (refer their catalogue)


-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
mathu.subramanian
Sent: Sunday, July 27, 2008 9:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:971] RE: 970] Consumable For UNS31254 weldoverlay on SA516
Gr. 70

Dear Friend,

You can use ER NiCrMo-10.

Regards,

S.Mathusoothanan

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Romio
Sent: 26 July, 2008 3:15 PM
To: Materials & Welding
Subject: [MW:970] Consumable For UNS31254 weldoverlay on SA516 Gr. 70


Has anybody experienced UNS31254 (P No. 8 Gr. 4.....chemi..20Cr 18Ni
6Mo) weldoverlay on SA516 Gr. 70
Can someone suggest the correct AWS class? If u can suggest the STRIP
consumable supplier for the smae it will be handful....

Romio


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...