Skip to main content

[MW:907] Re: Hardness variation on a temper bead welded F65 forging

 
Hi,
Actually as stated by me early we have first carried qualification in 5F position & later on 2F position.
I had mentioned 6 O'CLOCK & 12 O'CLOCK position for 5F position

Thanks for explaining the reason.

Regards
Sachin.Sankhe

On Tue, 08 Jul 2008 Bathula Raghuram(Mumbai - PIPING) wrote :
>It is some thing tricky, and difficult to evaluate the exact cause. Your
>assumptions regarding HI could be the reason for this at a particular
>position.
>
>But one thing is not clear to me, you welded this piece in rotating, how
>do you identify the 12'o clock position, where hardness is more?
>
>Yes your conclusions stated below will help us definitely in due course.
>
>
>
>Regarding your query on the previous statement the right vertical line
>is toe of the weld and left vertical line is toe of the surface temper
>reinforcing bead, this is mentioned to give a rough idea of surface
>temper bead placement, please note these surface temper beads may remain
>in place or may removed by grinding.
>
>
>
>  The in tempered HAZ as shown with arrow. Attachment in the previous
>post shows the same for tempering this arrow marked portion.
>
>
>
>________________________________
>
> From: sachin sankhe [mailto:sachin.sankhe@rediffmail.com]
>Sent: Monday, July 07, 2008 6:59 PM
>To: materials-welding@googlegroups.com
>Cc: Bathula Raghuram (Mumbai - PIPING)
>Subject: Re: [MW:904] Hardness variation on a temper bead welded F65
>forging
>
>
>
>
>Dear  Mr.Raghuram/Members,
>
>Let me apologise for not putting subject.
>
>Yes I had taken care as mentioned in your mail
>As u can see in attached figure that 8th pass was done on 6th pass.
>Distance between welding edge of  6th pass & 8th pass(i.e vertical
>distance in your mail sketch) was 3mm
>Yes preheating was done min. 150 deg.C & INTERPASS temp maintained at
>180-190 Deg.C
>
>Also why it give high hardness  on 12 O'CLOCK POSITION ONLY whereas it
>was accaptale in 6 O'CLOCK position
>
>Today I could see Macro of all specimen from DNV,Lab(Singapore).I
>compared weld profile of both 6'O CLOCK & 12 O'CLOCK specimen.I have
>noticed that fusion line in 12 O'CLOCK was not straight i.e When fusion
>line deviated far into base metal at that point hardness value was too
>high.So I think welder shall try  to maintain fusion line straight.
>Note that 2F position hardenss was OK
>
>So Conclusion is
>If hardness is critical to achieve
>
>1.Weld in such aposition that more Heat I/P can be done.In this case
>preferable position was 2F compare to 5F
>2.During capping avoid welding on base metal
>3.Grind 1/4th  or may be 1/2 of last fill passes before doing capping so
>that we can get good tempering of last fill pass
>4.Last Capping pass(Temper bead technique) shall be not that close to
>base metal so that it makes its own untempered HAZ in base metal
>
>Views on above concluded points are welcome
>
>I was not clear on your below statement can u be bit more clear on this
>
>"The distance between two vertical lines (as shown in attached sketch)
>shall be small enough that HAZ of reinforcing bead tempers all of the
>unaffected HAZ in the base metal, but not so small that it creates its
>own untempered region."
>
>Regards
>Sachin.Sankhe
>
>
>
>
>On Mon, 07 Jul 2008 Bathula Raghuram(Mumbai - PIPING) wrote :
> >Dear members
> >
> >Request to use appropriate subject line, thou the topic was very
> >interesting to discuss, it may be ignored by many in absence of an
> >appropriate subject line.
> >
> >
> >
> >There are chances that toe of the weld, where no tempering of HAZ has
> >occurred, in addition there is weld metal that is also not tempered, it
> >may be necessary to add a layer on top of the completed weld and grind
> >it off to get the desired results. This results in tempering of the
> >remaining untempered weld and HAZ. But be careful not to let this extra
> >tempering layer penetrates to base metal, if it, then you may create a
> >new untempered HAZ.
> >
> >The distance between two vertical lines (as shown in attached sketch)
> >shall be small enough that HAZ of reinforcing bead tempers all of the
> >unaffected HAZ in the base metal, but not so small that it creates its
> >own untempered region.
> >
> >(Remember) Cooling rate during welding : Thicker one cool faster than
> >thinner ones, with lower heat input cool rapidly than higher heat
>input,
> >cooler base material cool quicker than hotter ones (did you preheat
>this
> >one?)
> >
> >
> >
> >
> >
> >Invite more discussions, and active participation, irrespective of your
> >views whether right or wrong as only in discussion we can improve
> >
> >________________________________
> >
> > From: materials-welding@googlegroups.com
> >[mailto:materials-welding@googlegroups.com] On Behalf Of sachin sankhe
> >Sent: Saturday, July 05, 2008 6:52 PM
> >To: materials-welding@googlegroups.com
> >Subject:
> >
> >Dear Friends,
> >
> >Recently we have come across welding situation as mentioned below
> >
> >Details are as follows-
> >
> >1.Material used -API 5L X65 TO A694 F65
> >2.Position-5F
> >3.Welding Process-GTAW(Root,Hot)/SMAW(Fill, Cap)
> >4.Welding consumable-GTAW(ESAB OK 13.09),SMAW(E8016 GH4R)
> >5.Welding Technique-Temper Bead Technique
> >6Reference Codes-API1104/NACE MR0175/DNV 0S F101
> >7.Hardness Requiremnt as per Client Spec-248 HV10
> >8.Size(12" O.D X 27.3 mm Thk to 2" O.D X 8.7 mm Thk)
> >
> >Situation-
> >1.We carried out welding procedure qualification and sent for testing
> >2.Testing to be carried out-NICK BREAK & HARDNESS
> >3.Hardness  on capping pass (12 O'CLOCK )at forging side found above
>250
> >HV10
> >4.However at 6 O'CLOCK it was below 248HV10 & hence acceptable
> >5.Due to failure at 12 O'CLOCK POSITION,we decided to re-qualify.
> >6.This time we maintained high heat input(1.6-2.0 kJ/MM) on caping pass
> >at forging side
> >7.Hardness result again we found high at same location as
> >previous,however on 6 O'CLOCK position it was less then 248 HV10
> >8.Due to failure we decided along with client following option
> >  a)Two procedure to be qualified one in 5F position like prevoiusly
>but
> >this time we decided to rotate the pipe when welding capping pass on
> >forging side i.e Welding to be carried out only b/w 9-6-3 o'CLOCK
> >POSITION only.Thus avoiding welding in 12 O'CLOCK POSITION
> >Also we decided to use even higher heat i/p by using larger dia.
> >electrode (3.2 mm)in place of previoiuly used 2.5 mm electrode
> >  b)Secound procedure we decided to do in 2F position and maintaining
> >higher heat i/p(1.8-2.5 kj/mm)on capping pass(Forging side)
> >
> >9.After hardness testing for 5F position results on 12 O'CLOCK position
> >forging side again failed
> >10.However in 2F position it was satisfactory with same heat i/p as
>that
> >in 5F position
> >
> >Would like to know the reason of such behaviour
> >
> >Sachin.Sankhe
> >Engineer-Inspection
> >Aker Kvaerner-Malaysia
> >Mobile:012-2896901
> >Email1:Sachin.Sankhe@akerkvaerner.com
> >Email2:Sachin.sankhe@rediffmail.com
>
>
>
>
>
>
>
>
>
>>

Sachin.Sankhe
Engineer-Inspection
Aker Kvaerner-Malaysia
Mobile:012-2896901
Email1:Sachin.Sankhe@akerkvaerner.com
Email2:Sachin.sankhe@rediffmail.com


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...
Rediff Shopping